A Treatment Method for Improving the Comprehensive Quality of Wood Products
A treatment method and technology of wood products, applied in wood treatment, wood treatment details, radiation/wave wood treatment, etc., can solve problems such as water resistance, abrasion resistance, mold resistance, general treatment effect, human hazards, etc., to achieve anti-corrosion Good adhesion performance, improved corrosion resistance, and the effect of avoiding cracking
Image
Examples
Embodiment 1
[0024] A processing method for improving the comprehensive quality of wood products, comprising the following steps:
[0025] (1) Pretreatment of wood products: Grinding the newly made wood products to remove burrs on the surface;
[0026] (2) One-time treatment: After the treatment in step (1), the surface of the wood product is coated with a layer of water-based paint. After the coating is completed, the wood product is treated with ultraviolet radiation, and the wavelength of ultraviolet light is 200nm;
[0027] (3) Secondary treatment: Spray a layer of water-based paint on the surface of the wood product after the first treatment, and then carry out irradiation treatment on the wood product after the coating is completed. The total time of irradiation treatment is 50 minutes.
[0028] Further, the water-based paint in step (2) or step (3) consists of the following components in parts by weight: 60 parts of epoxy resin, 18 parts of acrylic acid, 10 parts of polyethylene gly...
Embodiment 2
[0039] A processing method for improving the comprehensive quality of wood products, comprising the following steps:
[0040] (1) Pretreatment of wood products: Grinding the newly made wood products to remove burrs on the surface;
[0041] (2) One-time treatment: After the treatment in step (1), the surface of the wood product is coated with a layer of water-based paint. After the coating is completed, the wood product is treated with ultraviolet radiation, and the wavelength of ultraviolet light is 210nm;
[0042] (3) Secondary treatment: Spray a layer of water-based paint on the surface of the wood product after the first treatment, and then carry out irradiation treatment on the wood product after the coating is completed. The total time of irradiation treatment is 55 minutes.
[0043]Further, the water-based paint in step (2) or step (3) consists of the following components in parts by weight: 65 parts of epoxy resin, 20 parts of acrylic acid, 12 parts of polyethylene glyc...
Embodiment 3
[0054] A processing method for improving the comprehensive quality of wood products, comprising the following steps:
[0055] (1) Pretreatment of wood products: Grinding the newly made wood products to remove burrs on the surface;
[0056] (2) One-time treatment: after the treatment in step (1), the surface of the wood product is coated with a layer of water-based paint, and after the coating is completed, the wood product is treated with ultraviolet radiation, and the wavelength of ultraviolet light is 220nm;
[0057] (3) Secondary treatment: Spray a layer of water-based paint on the surface of the wood product after the first treatment, and then carry out irradiation treatment on the wood product after the coating is completed. The total time of irradiation treatment is 60 minutes.
[0058] Further, the water-based paint in step (2) or step (3) consists of the following components in parts by weight: 70 parts of epoxy resin, 22 parts of acrylic acid, 14 parts of polyethylene...
PUM
Login to View More Abstract
Description
Claims
Application Information
- IPC
- B27M1/08; B27K5/00; C09D4/02; C09D4/06; C09D7/61; C09D7/62; C09D7/63; C09D7/65
- CPC
- B27K5/0055; B27M1/08; C09D4/06; C09D7/61; C09D7/62; C09D7/63; C09D7/65
- Inventors
- å¼ å¤§æ˜Œ