A technology of spraying material and roadway, which is applied in the field of preparation of roadway spraying material, can solve the problems of large amount of concrete rebound, serious environmental pollution, long gelation time, etc., to improve speed and quality, improve working environment, good economic benefits and The effect of social benefits
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0019] The invention discloses a roadway spraying material. The composition of the spraying material includes: white cement, quartz powder, titanium dioxide, polymer xanthan gum powder, adhesive and thixotropic agent, and their weight percentage is: 50:80 :9:33:14:14.
[0020] A kind of preparation method of roadway spraying material, described spraying material raw material is prepared by weight percentage each time with 5t product as base, mainly comprises the following steps:
[0021] 1) The polymer xanthan gum powder and the thixotropic agent with a weight percentage of 33:14 were added into a 2t automatic dry powder mixer with a power of 2.5KW and stirred for 5 minutes;
[0022] 2) Stop for 5 minutes after step 1) is completed, then add an adhesive with a weight percentage of 1:1 to the thixotropic agent into the feed port of a 2t automatic dry powder mixer with a power of 2.5KW and continue stirring for 5 minutes;
[0023] 3) At the same time, add white cement, quartz p...
Embodiment 2
[0028] A kind of preparation method of roadway spraying material, described spraying material raw material is prepared by weight percentage each time with 5t product as base, mainly comprises the following steps:
[0029] 1) Add 825Kg of polymer xanthan gum powder and 350Kg of anti-settling thixotropic agent 6650R into a 2t automatic dry powder mixer with a power of 2.5KW and stir for 5 minutes;
[0030] 2) Stop for 5 minutes after step 1) is completed, then add 350Kg of redispersible latex powder XY-6010 to the feeding port of a 2t automatic dry powder mixer with a power of 2.5KW and continue stirring for 5 minutes;
[0031] 3) At the same time, add 1250Kg of white cement, 2000Kg of quartz powder and 225Kg of titanium dioxide into a 6t automatic dry powder mixer with a power of 5.5KW and stir for 15 minutes;
[0032] 4) Add the mixed material stirred in step 2) into the 6t fully automatic dry powder mixer in step 3) and stir for another 15 minutes;
[0033] 5) Stop for 10 mi...
Embodiment 3
[0036] The construction site needs to have 0.6Mpa to 1.0MPa compressed air and tap water; the construction equipment for spraying materials is two 100L mixing barrels, one 10L plastic measuring cylinder, one ER50 pneumatic mixing gun, and one set of HY80L pressure spray tank (with safety valve, pressure regulating valve, etc.), one HYZ1.0 automatic air pressure long spray gun, one HYD1.0 automatic air pressure short gun, air pipes, joints, etc., and the staffing is 4 people;
[0037] The specific steps of the roadway spraying construction method are as follows:
[0038] Firstly, connect all the pneumatic tools firmly with the on-site air source. Secondly, pour 30L tap water into a 100L mixing tank with a 10L plastic measuring cylinder, then add a bag of 15Kg spray material, and then stir with an ER50 pneumatic mixing gun. Control the stirring at 300-500rpm for 5 minutes, then control the speed at 1500-2000rpm and stir for 10 minutes, pour the stirred slurry into the HY80L pres...