Antifreezing reflective coating and preparation method thereof
A technology of reflective paint and fluorescent powder, applied in the field of paint, can solve problems such as falling off of reflective stickers, hidden dangers of driving at night, difficult to find roadblock facilities, etc., and achieve the effect of avoiding cracking problems
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0053] The antifreeze reflective paint of the present invention consists of the following components in parts by weight:
[0054] 40 parts of polyvinyl butyral;
[0055] 18 parts of yttrium nitrate;
[0056] Magnetic powder 10 parts;
[0057] 6 parts of propylene glycol phenyl ether;
[0058] 6 parts zinc phosphate;
[0059] 6 parts of film-forming agent;
[0060] Phosphor powder 10 parts;
[0061] Thickener 4 parts;
[0062] 8 parts of barium nitrite;
[0063] 8 parts of sucrose fatty acid ester;
[0064] 40 parts of water.
[0065] When preparing, add polyvinyl butyral, yttrium nitrate, magnetic powder, barium nitrite, and sucrose fatty acid ester into water and stir for 30 minutes at 80°C, then add zinc phosphate and fluorescent powder and stir for 30 minutes, and finally add thickener and stir for 15 minutes. become.
Embodiment 2
[0067] The antifreeze reflective paint of the present invention consists of the following components in parts by weight:
[0068] 45 parts of polyvinyl butyral;
[0069] 20 parts of yttrium nitrate;
[0070] 15 parts of magnetic powder;
[0071] 8 parts of propylene glycol phenyl ether;
[0072] 5 parts zinc phosphate;
[0073] 4-8 parts of film-forming agent;
[0074] Phosphor powder 12 parts;
[0075] 3 parts of thickener;
[0076] 10 parts of barium nitrite;
[0077] 10 parts of sucrose fatty acid ester;
[0078] 30 parts of water.
[0079] When preparing, add polyvinyl butyral, yttrium nitrate, magnetic powder, barium nitrite, and sucrose fatty acid ester into water and stir for 30 minutes at 80°C, then add zinc phosphate and fluorescent powder and stir for 30 minutes, and finally add thickener and stir for 15 minutes. become.
Embodiment 3
[0081] The antifreeze reflective paint of the present invention consists of the following components in parts by weight:
[0082] 45 parts of polyvinyl butyral;
[0083] 20 parts of yttrium nitrate;
[0084] 15 parts of magnetic powder;
[0085] 5 parts of propylene glycol phenyl ether;
[0086] 5 parts zinc phosphate;
[0087] 8 parts of film-forming agent;
[0088] Phosphor powder 8 parts;
[0089] 5 parts of thickener;
[0090] 10 parts of barium nitrite;
[0091] 10 parts of sucrose fatty acid ester;
[0092] 50 parts of water.
[0093] When preparing, add polyvinyl butyral, yttrium nitrate, magnetic powder, barium nitrite, and sucrose fatty acid ester into water and stir for 30 minutes at 80°C, then add zinc phosphate and fluorescent powder and stir for 30 minutes, and finally add thickener and stir for 15 minutes. become.
[0094]The antifreeze reflective coating prepared by the above formula in the present invention can effectively reflect light in a dark envi...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com