Functional layer coating material of projection curtain, projection curtain and production method therefor
A technology of projection screen and functional layer, applied in the field of projection, can solve the problems of low brightness gain, narrow viewing angle, low brightness, etc., and achieve the effect of improving brightness and contrast, blocking water vapor invasion, and simple production method
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0041] A method for making a projection screen, comprising the following steps:
[0042] (1) Provide base layer, the material of base layer is PVC;
[0043] (2) A water vapor barrier layer is provided on one side of the base layer, and the material of the water vapor barrier layer includes olefin polymer, specifically ethylene homopolymer.
[0044] (3) Mix 70 parts of PVC resin, 40 parts of ethyl acetate and 22 parts of sizing agent, stir at 50-65°C for 20-60 minutes, then add 8 parts of citrate plasticizer and 4 parts of ultraviolet absorber in sequence And 2 parts of matting agent, ultrasonic high-speed dispersion, ultrasonic frequency is 20KHz, then add additives, stir for 20 to 40 minutes, then use a 400-mesh filter to filter under normal pressure, and then stand for 3 hours to obtain a functional layer coating;
[0045] Coating the functional layer coating on the side of the water vapor barrier layer away from the base layer.
[0046] Wherein, the auxiliary agent includ...
Embodiment 2
[0049] A method for making a projection screen, comprising the following steps:
[0050] (1) Provide a base layer, and the material of the base layer is PET;
[0051] (2) A water vapor barrier layer is provided on one side of the base layer, and the material of the water vapor barrier layer includes an olefin polymer, specifically a propylene homopolymer.
[0052] (3) Mix 80 parts of PVC resin, 50 parts of ethyl acetate and 15 parts of sizing agent, stir at 50-65°C for 20-60 minutes, then add 5 parts of citrate plasticizer and 8 parts of ultraviolet absorber in sequence And 1 part of matting agent, ultrasonic high-speed dispersion, ultrasonic frequency is 35KHz, then add additives, stir for 20 to 40 minutes, then use a 500-mesh filter to filter under normal pressure, and then stand for 5 hours to obtain a functional layer coating;
[0053] Coating the functional layer coating on the side of the water vapor barrier layer away from the base layer.
[0054] Wherein, the auxilia...
Embodiment 3
[0057] A method for making a projection screen, comprising the following steps:
[0058] (1) Provide base layer, the material of base layer is TPU (thermoplastic polyurethane elastomer rubber);
[0059] (2) A water vapor barrier layer is provided on one side of the base layer, and the material of the water vapor barrier layer includes an olefin polymer, specifically an ethylene-propylene copolymer.
[0060](3) Mix 75 parts of PVC resin, 45 parts of ethyl acetate and 18 parts of sizing agent, stir at 50-65°C for 20-60 minutes, then add 7 parts of citrate plasticizer and 6 parts of ultraviolet absorber in sequence And 1 part of matting agent, ultrasonic high-speed dispersion, ultrasonic frequency is 30KHz, then add additives, stir for 20 to 40 minutes, then use a 500-mesh filter to filter under normal pressure, and then stand for 4 hours to obtain a functional layer coating;
[0061] Coating the functional layer coating on the side of the water vapor barrier layer away from the...