A kind of beneficiation method of olivine pyroxene type ilmenite
A beneficiation method and ilmenite technology, applied in chemical instruments and methods, wet separation, solid separation, etc., can solve the problems of low raw ore, unfavorable flotation, unsatisfactory titanium concentrate grade and recovery rate, etc. Achieve the effect of reducing grade and improving grade
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0078] The first-stage iron beneficiation tailings (tailings of the first-stage grinding and magnetic separation in the iron beneficiation process) of the olivine-type ilmenite ore are treated with a slag screen with a diameter of 3 mm, and then the coarse-grained first-stage iron removal is carried out, and the magnetic field strength is 2000 o ster, get a first-stage iron removal concentrate and a first-stage iron removal tailings;
[0079] The first stage of iron removal tailings is subjected to a stage of strong magnetic roughing, the magnetic field strength is 7000 oersted, the rotating speed is 3r / min, the pulsation frequency is 300 times / min, and the stroke is 35mm, to obtain a stage of strong magnetic roughing concentrate and a stage of strong magnetic roughing. Magnetic roughing tailings;
[0080] The first stage of strong magnetic roughing tailings is subjected to a stage of strong magnetic sweeping (magnetic field strength 5000 oersteds, swivel speed 3r / min, pulsati...
Embodiment 2
[0129] The first-stage iron beneficiation tailings (tailings of the first-stage grinding and magnetic separation in the iron beneficiation process) of the olivine-type ilmenite ore are treated with a slag screen with a diameter of 3 mm, and then the coarse-grained first-stage iron removal is carried out. The magnetic field strength is 1000 o ster, get a first-stage iron removal concentrate and a first-stage iron removal tailings;
[0130] The first stage of iron removal tailings is subjected to a stage of strong magnetic roughing, the magnetic field strength is 5000 oersted, the rotating speed is 3r / min, the pulsation frequency is 300 times / min, and the stroke is 35mm to obtain a stage of strong magnetic roughing concentrate and a stage of strong magnetic roughing. Magnetic roughing tailings;
[0131] The first stage of strong magnetic roughing tailings is subjected to a stage of strong magnetic sweeping (magnetic field strength 3000 oersteds, swivel speed 3r / min, pulsation fr...
Embodiment 3
[0156] The first-stage iron beneficiation tailings (tailings of the first-stage grinding and magnetic separation in the iron beneficiation process) of the olivine-type ilmenite ore are treated with a slag screen with a diameter of 3 mm, and then the coarse-grained first-stage iron removal is carried out. The magnetic field strength is 3000 o'clock. ster, get a first-stage iron removal concentrate and a first-stage iron removal tailings;
[0157] The first stage of iron removal tailings is subjected to a stage of strong magnetic roughing, the magnetic field strength is 10,000 Oersted, the rotating speed is 3r / min, the pulsation frequency is 300 times / min, and the stroke is 35mm to obtain a stage of strong magnetic roughing concentrate and a stage of strong magnetic separation. Magnetic roughing tailings;
[0158] The first stage of strong magnetic roughing tailings is subjected to a stage of strong magnetic sweep selection (magnetic field strength 8000 oersted, swivel rotation ...