An amino silicone oil and emulsion technology, which is applied in pharmaceutical formulations, cosmetic preparations, cosmetic preparations, etc., can solve problems, affect the use effect of products, high viscosity and other problems, achieve a simple emulsification process, facilitate promotion and production, and maintain suppleness. effect of moisturizing and moisturizing
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0028] A preparation method of amino silicone oil emulsion, comprising the following steps:
[0029] (1) Take amopolydimethylsiloxane, alcohol ether glycoside, glucose amide, ethylene glycol monobutyl ether, trifluoromethyl maleic anhydride, acetic acid and water;
[0030] (2) Add amodimethicone, alcohol ether glycoside, glucose amide and trifluoromethyl maleic anhydride into the reaction vessel, stir at 4000rpm at 60°C for 90min, then add ethylene glycol monobutyl Continue to stir the ether for 60 minutes, add water, and stir for 45 minutes at a speed of 500 rpm;
[0031] (3) Add acetic acid to the system obtained in step (2) to adjust the pH to 5.0-7.0, and stir evenly at a speed of 300 rpm to obtain the amino silicone oil emulsion;
[0032] Wherein, the amino silicone oil emulsion includes the following components in weight percentage: 35% of amodimethicone, 4% of alcohol ether glycoside, 2% of glucose amide, 4% of ethylene glycol monobutyl ether, trifluoroform Base malei...
Embodiment 2
[0034] A preparation method of amino silicone oil emulsion, comprising the following steps:
[0035] (1) Take amopolydimethylsiloxane, alcohol ether glycoside, glucose amide, ethylene glycol monobutyl ether, trifluoromethyl maleic anhydride, acetic acid and water;
[0036] (2) Add amodimethicone, alcohol ether glycoside, glucose amide and trifluoromethyl maleic anhydride into the reaction vessel, stir at 4000rpm at 60°C for 90min, then add ethylene glycol monobutyl Continue to stir the ether for 60 minutes, add water, and stir for 45 minutes at a speed of 500 rpm;
[0037] (3) Add acetic acid to the system obtained in step (2) to adjust the pH to 5.0-7.0, and stir evenly at a speed of 300 rpm to obtain the amino silicone oil emulsion;
[0038] Wherein, the amino silicone oil emulsion includes the following components in weight percentage: 35% of amodimethicone, 4.8% of alcohol ether glycoside, 1.2% of glucose amide, 4% of ethylene glycol monobutyl ether, trifluoromethyl Base...
Embodiment 3
[0040] A preparation method of amino silicone oil emulsion, comprising the following steps:
[0041] (1) Take amopolydimethylsiloxane, alcohol ether glycoside, glucose amide, ethylene glycol monobutyl ether, trifluoromethyl maleic anhydride, acetic acid and water;
[0042] (2) Add amodimethicone, alcohol ether glycoside, glucose amide and trifluoromethyl maleic anhydride into the reaction vessel, stir at 4000rpm at 60°C for 90min, then add ethylene glycol monobutyl Continue to stir the ether for 60 minutes, add water, and stir for 45 minutes at a speed of 500 rpm;
[0043] (3) Add acetic acid to the system obtained in step (2) to adjust the pH to 5.0-7.0, and stir evenly at a speed of 300 rpm to obtain the amino silicone oil emulsion;
[0044] Wherein, the amino silicone oil emulsion includes the following components in weight percentage: 35% of amodimethicone, 5% of alcohol ether glycoside, 1% of glucose amide, 4% of ethylene glycol monobutyl ether, trifluoroform Base malei...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com