Composite thermal insulation building block for building
A composite thermal insulation and building block technology, which is applied in the direction of buildings, building components, building materials, etc., can solve the problems of low structural strength and achieve good stability, reduce cracks, and simple connection methods
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0035] Such as figure 1 and figure 2 As shown, a building composite thermal insulation block includes block one 1 and block two 2, the two sides of block one 1 are symmetrically provided with tapered grooves 3, and the bottom of the tapered groove 3 is provided with a semi-arc slot 9, and the half-arc A cylinder 6 is arranged in the shape card groove 9, and a protrusion 8 matched with the tapered groove 3 is arranged on both sides of the block two 2 .
[0036] Square hole 1 4 is arranged symmetrically on both sides of the middle of block 1 and block 2, and square hole 2 5 is arranged in the middle; square hole 1 on block 1 is filled with thermal insulation material, and square hole 2 on block 2 5 is filled with heat-insulating material, and the material of the cylinder 6 arranged in the semi-arc-shaped slot 9 is heat-insulating material, and the heat-insulating material in the present application is polystyrene foam plastics, wherein wherein block 1 and block 2 are laid stru...
Embodiment 2
[0051] Embodiment 2 differs from Embodiment 1 in that:
[0052] Block 1 and Block 2 2 are prepared from thermal insulation mortar, which is made of the following raw materials in parts by weight: 95 parts of 42.5 Portland cement, 64 parts of aggregate, 11 parts of porous filler, reinforcing fiber 5.4 parts, 2.2 parts of gypsum whiskers, 0.6 parts of polycarboxylate superplasticizer, 42 parts of water.
[0053] Reinforcement fibers are steel fibers and straw fibers mixed at a weight ratio of 1:0.6, in which steel fibers have a diameter of 5-20 μm and a length of 2-3 mm, and straw fibers are chopped fibers made of crushed corn stalks, with a length of 3-4 cm , a width of 0.5-1cm.
[0054] The aggregate is made by mixing waste concrete, steel slag and waste rubber particles in a weight ratio of 2:1:0.6.
[0055] Aggregate is pretreated before use, and the specific pretreatment steps are:
[0056] 1) After the waste concrete is crushed and steel slag is placed in 2.5 times the ...
Embodiment 3
[0061] Embodiment 3 differs from Embodiment 1 in that:
[0062] Block 1 and Block 2 2 are prepared from thermal insulation mortar, which is made of the following raw materials in parts by weight: 98 parts of 42.5 Portland cement, 68 parts of aggregate, 11.5 parts of porous filler, reinforcing fiber 5.8 parts, 2.5 parts of gypsum whiskers, 0.8 parts of polycarboxylate superplasticizer, 44 parts of water.
[0063] Reinforcing fibers are steel fibers and straw fibers mixed at a weight ratio of 1:0.8, in which steel fibers have a diameter of 5-20μm and a length of 2-3mm, and straw fibers are chopped fibers made of crushed corn stalks, with a length of 3-4cm , a width of 0.5-1cm.
[0064] The aggregate is made by mixing waste concrete, steel slag and waste rubber particles in a weight ratio of 2:1:0.7.
[0065] Aggregate is pretreated before use, and the specific pretreatment steps are:
[0066] 1) Put waste concrete and steel slag in 2.5 times the weight of 2.5wt% lime water an...
PUM
| Property | Measurement | Unit |
|---|---|---|
| particle diameter | aaaaa | aaaaa |
| length | aaaaa | aaaaa |
| diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
Login to View More 