Point-to-point directional treatment and utilization method for waste incineration fly ash
A waste incineration fly ash, point-to-point technology, applied in chemical instruments and methods, landfill technology, cement production, etc. problems such as solidification and removal of pollutants such as chlorine and other pollutants
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0099] A method for point-to-point directional disposal and utilization of waste incineration fly ash, the method comprises the following steps:
[0100] S1 solidifies the waste incineration fly ash of the waste incineration plant to form a geopolymer solidified body; S2 makes the geopolymer solidified body into a geopolymer solidified agent The specific implementation steps are as follows:
[0101] S1.1 Take 80% mass percentage of waste incineration fly ash as aggregate, first perform water washing pretreatment and 850-1000 ℃ high temperature pretreatment, the specific steps of pretreatment are: mix water and waste incineration fly ash according to the liquid-solid mass ratio In a ratio of 2:1, the waste incineration fly ash is mixed with water, stirred at a slow speed for 0.5-6 hours, and then dehydrated and dried; then the waste incineration fly ash after pretreatment and drying is washed in a high-temperature furnace at 850-1000 ℃. After heating for 1-4 hours, the pretreat...
Embodiment 2
[0108] A method for point-to-point directional disposal and utilization of waste incineration fly ash, the method comprises the following steps:
[0109] S1 solidifies the waste incineration fly ash of the waste incineration plant to form a geopolymer solidified body; S2 makes the geopolymer solidified body into a geopolymer solidified agent The specific implementation steps are as follows:
[0110] S1.1 Take 70% mass percentage of waste incineration fly ash as aggregate, and firstly carry out water washing pretreatment and high temperature pretreatment at 850-1000℃. The specific steps of pretreatment are: mix water and waste incineration fly ash according to the liquid-solid mass ratio In a ratio of 3:1, the waste incineration fly ash is mixed with water, stirred at a slow speed for 0.5-6 hours, then dehydrated and dried; then in a high temperature furnace, the waste incineration fly ash after pretreatment and drying is washed at 850-1000 ℃. After heating for 1-4 hours, the p...
Embodiment 3
[0117] A method for point-to-point directional disposal and utilization of waste incineration fly ash, the method comprises the following steps:
[0118] S1 solidifies the waste incineration fly ash of the waste incineration plant to form a geopolymer solidified body; S2 makes the geopolymer solidified body into a geopolymer solidified agent The specific implementation steps are as follows:
[0119] S1.1 Take 60% mass percentage of waste incineration fly ash as aggregate, first perform water washing pretreatment and 850-1000 ℃ high temperature pretreatment; the specific steps of pretreatment are: mix water and waste incineration fly ash according to the liquid-solid mass ratio In a ratio of 4:1, the waste incineration fly ash is mixed with water, stirred at a slow speed for 0.5-6 hours, and then dehydrated and dried; then the waste incineration fly ash after pretreatment and drying is washed in a high-temperature furnace at 850-1000 ℃. After heating for 1-4 hours, the pretreat...