A technology for electrolytic manganese metal and ammonia gas, which is applied in the field of electrolytic manganese metal, can solve the problems of environmental protection adverse effects, increase the time for workers to prepare ammonia water, increase labor load, etc., so as to avoid ammonia gas overflowing and pollute the environment, and save ammonia water preparation The effect of saving time and reducing labor load
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] Embodiment 1, the method for producing electrolytic manganese metal by neutralizing and removing iron in ammonia gas instead of ammonia, the steps are as follows:
[0019] (1), in the leaching stage, inject 170M into the leaching tank 3 Anolyte, stirred for 10 minutes, analyzed for Mn 2+ 、H + , let the anolyte content Mn 2+ : 14g / L, H + : 35g / L, (NH 4 ) 2 SO 4 : 110g / L.
[0020] (2), according to the anolyte content, by formula (1), (2) and (3), calculate the sulfuric acid and mineral powder weight that needs to input, here two ore weight ratio (manganese dioxide ore: manganese carbonate ore) 0.2, acid ore Ratio (total acid quantity: total ore quantity) 0.4, the result calculates 4.76 tons of sulfuric acid (concentration 98%), 22.12 tons of manganese carbonate ore (ΣMn15%, ΣFe6.4%), 4.424 tons of manganese dioxide ore (ΣMn48%, ∑Fe6.0%).
[0021] (3) Add the calculated required sulfuric acid from the sulfuric acid metering tank to the compound tank. At this time...
example 2
[0028] Example 2: Utilize ammonia to replace the method for neutralizing and removing iron in ammonia to produce electrolytic metal manganese, the steps are as follows:
[0029] (1), in the leaching stage, inject 170M into the leaching tank 3 Anolyte, stirred for 10 minutes, analyzed for Mn 2+ 、H + , let the anolyte content Mn 2+ : 14g / L, H + : 35g / L, (NH 4 ) 2 SO 4 : 110g / L.
[0030] (2), according to the anolyte content, calculate the sulfuric acid and ore powder weight that needs to input by formula (1), (2) and (3), here two ore weight ratio (manganese dioxide ore: manganese carbonate ore) 0.25, acid ore Ratio (total acid amount: total ore amount) 0.5, the result calculates 6.78 tons of sulfuric acid (concentration 98%), 20.152 tons of manganese carbonate ore (∑Mn15%, ∑Fe6.4%), 5.038 tons of manganese dioxide ore (∑Mn48%, ∑Fe6.0%).
[0031] The following steps are the same as in Example 1.
example 3
[0032] Example 3: Utilize ammonia to replace the method for neutralizing and removing iron in ammonia to produce electrolytic manganese metal, the steps are as follows:
[0033] (1), in the leaching stage, inject 170M into the leaching tank 3Anolyte, after stirring for 10 minutes, analyze Mn 2+ 、H + , let the anolyte content Mn 2+ : 14g / L, H + : 35g / L, (NH 4 ) 2 SO 4 : 110g / L.
[0034] (2), according to the anolyte content, calculate the sulfuric acid and ore powder weight that needs to drop in according to formula (1), (2) and (3), here two ore weight ratios are by (manganese dioxide ore: manganese carbonate ore) 0.3, acid ore Calculated by (total acid amount: total mineral amount) 0.6, the result is 8.41 tons of sulfuric acid (concentration 98%), 18.19 tons of manganese carbonate (∑Mn15%, ∑Fe6.4%), 5.457 tons of manganese dioxide ore (∑Mn48%, ΣFe6.0%).
[0035] The following steps are the same as in Example 1.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology