A countertop made of acrylic material coated with pvc wood-plastic board
A technology using acrylic and countertops, applied in applications, household appliances, devices for coating liquids on surfaces, etc., can solve the problems of easy deformation, reduce costs, reduce the weight of acrylic materials, etc., to reduce density, reduce production costs, The effect of improving impact resistance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0016] Take polymethyl methacrylate, high white filler aluminum hydroxide, titanium dioxide, pigments, color particles, accelerators, and stabilizers.
[0017] The first step: React polymethyl methacrylate, high white filler aluminum hydroxide, titanium dioxide, pigment, color particles and accelerator stabilizer in a negative pressure vacuum reactor at a pressure of -0.1MPa and a temperature of 30°C according to the formula ratio 40 minutes.
[0018] The second step: place the cladding slurry in a vacuum device for treatment at a pressure of -0.1 MPa for 1 minute.
[0019] The third step: use the molding equipment to coat the vacuum-treated coating slurry on the surface of the processed PVC honeycomb panel substrate.
[0020] Step 4: Place the painted decorative slab in a heat treatment device at a temperature of 40° C. for 40 minutes.
[0021] Step 5: Surface sanding, polishing, and trimming the stably formed decorative panels to make decorative panels with specifications ...
Embodiment 2
[0023] Take polymethyl methacrylate, high white filler aluminum hydroxide, titanium dioxide, pigments, color particles, accelerators, and stabilizers.
[0024] The first step: React polymethyl methacrylate, high white filler aluminum hydroxide, titanium dioxide, pigment, color particles and accelerator stabilizer in a negative pressure vacuum reactor at a pressure of -0.15MPa and a temperature of 35°C according to the formula ratio 45 minutes.
[0025] The second step: place the cladding slurry in a vacuum device for treatment at a pressure of -0.15 MPa for 6 minutes.
[0026] The third step: use the molding equipment to coat the vacuum-treated coating slurry on the surface of the processed PVC honeycomb panel substrate.
[0027] Step 4: Place the painted decorative slab in a heat treatment device at a temperature of 45° C. for 47 minutes.
[0028] Step 5: Surface sanding, polishing, and trimming the stably formed decorative panels to make decorative panels with specificatio...
PUM
Login to View More Abstract