Energy-saving, environment-friendly and water-soluble artificial marble multi-colour paint and preparation method thereof
A technology of imitating marble and colorful paint, applied in the field of building decoration materials, can solve the problems of loss of safety and environmental protection, no heat preservation and energy saving effect, human health hazards, etc. Production requirements, the effect of short process steps
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0030] A) Preparation of color particle components:
[0031] 31 parts of deionized water, 0.2 parts of preservatives, 0.2 parts of defoamers, 1.2 parts of dispersants, 0.15 parts of wetting agents, 1.5 parts of propylene glycol as antifreezing agent, 9 parts of pigments and fillers and 8 parts of functional materials are put into a container equipped with a stirring device and stirred evenly. The container in this embodiment is a dispersion kettle. After the feeding is finished, the stirring speed is changed to 3000n / min, and the stirring time is 30min, so that the aforementioned materials are dispersed into the slurry and in a uniform state. The above process is the hydration and aging process, and then the synthetic resin weighed by weight is put into 40 parts of emulsion, 0.1 part of defoamer, 3.5 parts of film-forming aid and 2 parts of thickener, and continue to stir for 15 minutes at a stirring speed of 1000n / min to obtain the color particle base material, and then mix t...
Embodiment 2
[0039] A) Preparation of color particle components:
[0040] 42 parts of deionized water, 0.1 part of preservative, 0.4 part of defoamer, 0.9 part of dispersant, 0.7 part of wetting agent, 2 parts of polypropylene glycol as an antifreeze agent, and 5 parts of pigments and fillers are weighed in parts by weight. and 20 parts of functional materials are put into a container with a stirring device and stirred evenly. During the feeding process, the stirring speed of the stirring device is controlled to 600n / min, and after the feeding is completed, the stirring speed is changed to 2000n / min. The stirring time is 50min, then drop into the container by weight 25 parts of synthetic resin emulsion, 0.2 part of defoamer, 2 parts of film-forming aid and 0.5 part of thickener, and under the stirring speed of 1500n / min Stir for 10 minutes to obtain the color particle base material, then put the color particle base material and pre-gel into the shearing and dispersing device at a weight ra...
Embodiment 3
[0048] A) Preparation of color particle components:
[0049] 36.5 parts of deionized water, 0.4 parts of preservatives, 0.25 parts of defoamers, 0.6 parts of dispersants, 1 part of wetting agent, 2.3 parts of polypropylene glycol as antifreeze, and 12 parts of pigments and fillers weighed in parts by weight and 14 parts of functional materials were put into a container equipped with a stirring device and stirred evenly. During the feeding process, the stirring speed of the stirring device was controlled to 550n / min, and after the feeding was completed, the stirring speed was changed to 2500n / min. The stirring time was 40min, then drop into the container by weight 33 parts of synthetic resin emulsion, 0.2 part of defoamer, 0.5 part of film-forming aid and 3.5 parts of thickener, and under the stirring speed of 1250n / min Stir for 5 minutes to obtain the color particle base material, and then put the color particle base material and pre-gel into the shear dispersion device at a w...