Method for producing pigment red 48:2 with excellent heat resistance and migration resistance

A production method and migration-resistant technology, applied in chemical instruments and methods, organic dyes, color lakes, etc., can solve the problems of low coloring power of pigments and decline in heat resistance, achieve transparency and coloring power, and improve heat resistance , design reasonable effect

Active Publication Date: 2013-11-13
CROWN CHEMICAL CORP
View PDF4 Cites 12 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

The coloring power of the pigment prepared by it is low, and due to the introduction of rosin, the heat resistance is reduced. It can withstand heat at 210°C*5min in PP, and the migration on PU is below grade 3.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Method for producing pigment red 48:2 with excellent heat resistance and migration resistance
  • Method for producing pigment red 48:2 with excellent heat resistance and migration resistance

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0024] 1) Add 200Kg of 6-chloro-4-aminotoluene-3-sulfonic acid sodium salt into the reaction kettle, add 1800Kg of water, heat up to 90-95°C, stir for 10-20min; add concentrated hydrochloric acid within 5min, and stir for more than 30min ; Then slowly add 250Kg of 30% sodium nitrite aqueous solution at 0°C to carry out the diazotization reaction and stir for 1 hour; then add 800Kg of 30% calcium chloride aqueous solution to the above diazonium solution;

[0025] 2) Add 2000Kg of water, 285Kg of liquid caustic soda and 160Kg of 2,3 acid into the coupling reaction kettle, and stir at a temperature of 40-50°C to obtain a clear liquid;

[0026] 3) Inject the diazo solution into the coupling reaction kettle at 12-15°C for coupling reaction, stir for 3 hours after adding the diazo solution; adjust the pH value of the reaction solution to 7.0, add 2Kg CH-M8, 4Kg Add O-15 into 400Kg water and heat it up to above 90°C to dissolve it, then slowly add it dropwise to the above reaction so...

Embodiment 2

[0028] 1) Add 200Kg of 6-chloro-4-aminotoluene-3-sulfonic acid sodium salt into the reaction kettle, add 1800Kg of water, heat up to 90-95°C, stir for 10-20min; add concentrated hydrochloric acid within 5min, and stir for more than 30min Then slowly add 250Kg of 30% sodium nitrite aqueous solution at 5°C to carry out the diazotization reaction and stir for 1 hour; then add 1000Kg of 30% calcium chloride aqueous solution to the above diazonium solution;

[0029] 2) Add 2000Kg of water, 285Kg of liquid caustic soda and 180Kg of 2,3 acid into the reaction kettle, stir at a temperature of 40-50°C to obtain a clear liquid;

[0030] 3) Inject the diazo solution into the coupling reaction kettle at 12-15°C for coupling reaction, stir for 3 hours after adding the diazo solution; adjust the pH value of the reaction solution to 7.0, mix 10Kg CH-3A, 10Kg Add O-9 to 400Kg water and heat it up to above 90°C to dissolve it, then slowly add it dropwise to the above reaction solution, stir fo...

Embodiment 3

[0032] 1) Add 200Kg of 6-chloro-4-aminotoluene-3-sulfonic acid sodium salt into the reaction kettle, add 1800Kg of water, heat up to 90-95°C, stir for 10-20min; add concentrated hydrochloric acid within 5min, and stir for more than 30min ; Then slowly add 250Kg of 30% sodium nitrite aqueous solution at 0°C to carry out the diazotization reaction and stir for 1 hour; then add 1200Kg of 30% calcium chloride aqueous solution to the above diazonium solution;

[0033] 2) Add 2000Kg of water, 285Kg of liquid caustic soda and 200Kg of 2,3 acid into the reaction kettle, stir at a temperature of 40-50°C to obtain a clear liquid;

[0034] 3) Inject the diazo solution into the coupling reaction kettle at 12-15°C for coupling reaction, and stir for 3 hours after adding the diazo solution; after adjusting the pH value of the reaction solution to 7.0, mix 12Kg CH-2C, 18Kg Add MOA-3 into 400Kg water and heat it up to above 90°C to dissolve it, then slowly add it dropwise to the above reactio...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention relates to a method for producing a pigment red 48:2 with excellent heat resistance and migration resistance and belongs to the technical field of fine chemical industries. The method comprises the following process steps of: under an acidic condition, carrying out stirring diazotization reaction on 6-chloro-4-aminotoluene-3-sodium sulfonate and sodium nitrite for 1 hour, then, adding calcium chloride aqueous solution, and continuously carrying out stirring reaction; after the reaction is ended, adding material liquid into a clear alkaline solution of 2-hydroxy-3-naphthoic acid, so as to carry out coupling reaction; and after the reaction is ended, adjusting the pH value of a reaction solution to 7.0, then, adding a mixed assistant aqueous solution into the reaction solution so as to carry out surface modification, then, heating the reaction solution to 95-100 DEG C, carrying out heat-preserved reaction, then, adding water for cooling to below 60 DEG C, filtering, washing with water and drying, thus obtaining the pigment red 48:2. The method has the advantages that the dispersity, heat resistance, solvent resistance and fluidity of the pigment can be improved remarkably, and the coloring effect of the pigment can be improved effectively.

Description

technical field [0001] The invention belongs to the technical field of fine chemicals, and in particular relates to a production method of Pigment Red 48:2 with excellent heat resistance and migration resistance. Background technique [0002] 6-Chloro-4-aminotoluene-3-sulfonic acid sodium salt (referred to as sodium 2B acid) is an important organic pigment intermediate. C.I.P.R.48:2 (sunfast red BBC) toner synthesized as a diazo component is bluish red, widely used in hard or soft PVC, LLDPE, LDPE, HDPE, PP plastic systems, and in rubber and PU Also applies in . [0003] C.I.P.R.48: 2 The traditional industrial production method is: after 2B sodium acid and water are purified at high temperature, acid precipitation with hydrochloric acid to form a salt, adding sodium nitrite aqueous solution for diazotization, the diazonium salt and the coupling component 2,3 acid Carry out coupling reaction, and then react with calcium chloride to transform into calcium salt lake, which i...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
IPC IPC(8): C09B67/20C09B67/36C09B63/00
Inventor 杨宗泽徐亮陈奇文
Owner CROWN CHEMICAL CORP