Real stone paint and preparation method thereof
A technology of real stone paint and dispersant, applied in the direction of coating, etc., can solve the problems of poor flexibility, difficult manual cleaning, easy deformation, etc., and achieve the effect of excellent flexibility
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0032] A real stone paint prepared from the following raw materials: 80.0kg of water, 3.0kg of ethylene glycol, 10.0kg of BYK-156 dispersant, 1.0kg of Deqian W-18 wetting agent, Dow ER-30M hydroxyethyl Base cellulose 4.0kg, Dow AMP-95PH regulator 4.0kg, silica sol 10.0kg, BASF SC138 elastic emulsion 30.0kg, BASF 296D-S styrene-acrylic emulsion 90.0kg, 20-40 mesh natural colored sand fine sand 60.0kg, 40-80 mesh natural colored sand medium sand 240.0kg, 80-120 mesh natural colored sand coarse sand 400.0kg, real stone varnish rock flakes of various colors 50.0kg, Eastman Texanol film-forming aid 10.0kg, BYK-024 defoamer 4.0kg, Deqian MB-11 preservative 4.0kg.
[0033] The preparation method of the real stone paint provided by the present embodiment 1 may further comprise the steps:
[0034] 1. In the real stone paint production equipment, add water 80.0kg, ethylene glycol 3.0kg, BYK-156 dispersant 10.0kg, Deqian W-18 wetting agent 1.0kg and Dow ER-30M hydroxyethyl Cellulose 4....
Embodiment 2
[0039] A real stone paint prepared from the following raw materials: 120.0kg of water, 17.0kg of ethylene glycol, 1.0kg of Dow H-30A dispersant, 0.2kg of BYK-310 wetting agent, and 0.2kg of Dow ER-30M hydroxyethyl Base cellulose 0.2kg, Deqian DMAE water-based amine neutralizer 0.2kg, silica sol 40.0kg, BASF SC138 elastic emulsion 50.0kg, BASF 296D-S styrene-acrylic emulsion 20.0kg, 20-40 mesh natural colored sand fine sand 40.0kg , 160.0kg medium sand of 40-80 mesh natural colored sand, 480.0kg natural colored sand coarse sand of 80-120 mesh, 70.0kg rock flakes of various colors, Eastman Texanol film-forming aid 1.0kg, BYK-033 defoaming agent Antiseptic 0.2kg, Deqian MB-16 preservative 0.2kg.
[0040] The preparation method of the real stone paint provided by the present embodiment 2 may further comprise the steps:
[0041] 1. In the real stone paint production equipment, add 120.0kg of water, 17.0kg of ethylene glycol, 1.0kg of Dow H-30A dispersant, 0.2kg of BYK-310 wetting ag...
Embodiment 3
[0046] A real stone paint prepared from the following raw materials: 106.5kg of water, 10.0kg of ethylene glycol, 5.0kg of Godix P-90 dispersant, 0.5kg of Dow X-405 wetting agent, 0.5kg of Dow ER-30M hydroxyl Ethyl cellulose 2.0kg, camine328 multifunctional additive 2.0kg, silica sol 25kg, BASF SC138 elastic emulsion 40.0kg, BASF 296D-S styrene-acrylic emulsion 50.0g, 20~40 mesh natural colored sand fine sand 50.0kg, 40~ 80 mesh natural colored sand medium sand 200.0kg, 80~120 mesh natural colored sand coarse sand 440.0kg, real stone varnish rock flakes of various colors 60.0kg, Eastman Texanol film-forming aid 5.0kg, Nopco SN-NXZ defoamer 2.0 kg, Rohm and Haas LXE preservative 2.0kg.
[0047] The preparation method of the real stone paint provided by the present embodiment 3 may further comprise the steps:
[0048] 1. In the genuine stone paint production equipment, add water 106.5kg, ethylene glycol 10.0kg, Godix P-90 dispersant 5.0kg, Dow X-405 wetting agent 0.5kg and Dow ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com