Novel low-cost production process of lithium ion battery PE (polyethylene) diaphragm
A lithium-ion battery, low-cost technology, applied in the direction of battery pack parts, circuits, electrical components, etc., can solve the problems of increasing production cost investment, low first-time pass rate of products, etc., and achieve the effect of reducing production costs
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
preparation example Construction
[0026] The present invention, a kind of preparation method of novel low-cost lithium-ion battery PE diaphragm, comprises the following steps:
[0027] Step 1, batching step: weigh 15-50% of polyethylene and 50-85% of organic solvent according to the weight percentage. The organic solvent of the present invention is preferably kerosene or decahydronaphthalene, and polyethylene and kerosene or decahydronaphthalene are fully mixed. Mixture A is obtained;
[0028] Step 2. Extrusion and metering steps: pass the mixture A in step 1 through a twin-screw extruder with a diameter of 96mm, an aspect ratio of 52, and a temperature of 130°C to obtain a high-temperature melt, and the high-temperature melt is accurately obtained by a melt pump Feed into the die head after metering;
[0029] Step 3, casting step: the high-temperature melt sent into the die in step 2 flows out from the slit of the die, and the high-temperature melt flowing out of the slit of the die passes through the temper...
Embodiment 1
[0035] A preparation method of a novel low-cost lithium-ion battery PE diaphragm, comprising the following steps:
[0036] Step 1. Ingredients: Weigh 70Kg of polyethylene powder and 396.67Kg of decahydronaphthalene, respectively, and pour them into the stirring tank (the stirrer is in the form of double ribbons) for full stirring to obtain the mixture A, which is set aside;
[0037] Step 2. Extrusion and metering steps: Mixture A passes through a twin-screw extruder with a diameter of 96mm, an aspect ratio of 52, and a temperature of 130°C to obtain a uniform high-temperature melt, and the high-temperature melt is accurately metered by a melt pump before entering In the die head;
[0038] Step 3, casting step: the high-temperature melt flowing out from the slit of the die head passes through four chilling rollers with temperatures of 20°C-30°C-30°C-30°C in sequence to obtain extruded cast pieces;
[0039] Step 4. Stretching step: Extrude the cast sheet into a bidirectional sy...
Embodiment 2
[0044] Step 1. Ingredients: Weigh 70Kg of polyethylene powder and 70Kg of decahydronaphthalene respectively, and pour them together into the stirring tank (the stirrer is in the form of double ribbons) for full stirring to obtain the mixture A, which is set aside;
[0045] Step 2. Extrusion and metering steps: Mixture A passes through a twin-screw extruder with a diameter of 96mm, an aspect ratio of 52, and a temperature of 130°C to obtain a uniform high-temperature melt, and the high-temperature melt is accurately metered by a melt pump before entering In the die head;
[0046] Step 3, casting step: the high-temperature melt flowing out from the slit of the die head passes through four chilling rollers with temperatures of 20°C-30°C-30°C-30°C in sequence to obtain extruded cast pieces;
[0047]Step 4. Stretching step: Extrude the cast sheet into a bidirectional synchronous stretching machine to obtain an oil-containing film with a longitudinal draw ratio of 4.5 times and a tr...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com