Copper molybdenum separation flotation agent and using method thereof

A flotation agent, copper and molybdenum technology, applied in flotation, solid separation, etc., can solve the problems of chemical wastewater COD exceeding the standard, environmental problems, etc., achieve the effect of small impact, good effect, and reduce usage

Active Publication Date: 2014-06-25
TIBET HUATAILONG MINING DEV
View PDF5 Cites 15 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0003] For the recovery of molybdenum from copper-molybdenum ores, a lot of research work and practice have been carried out at home and abroad, most of which use the separation technology of copper-inhibiting and floating molybdenum, but the copper-inhibiting inhibitors and floating molybdenum collectors used are mostly single drugs , such as sodium sulfide, sodium cyanide, kerosene, etc. However, when a single drug is used, the dosage needs to be large to separate completely, which causes the COD of the pharmaceutical wastewater to exceed the standard and brings environmental problems

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Copper molybdenum separation flotation agent and using method thereof
  • Copper molybdenum separation flotation agent and using method thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0026] Carry out copper molybdenum separation to obtain the technological process of copper concentrate and molybdenum concentrate as follows:

[0027] (A) Prepare inhibitors and collectors respectively, wherein the inhibitors are prepared from the following components: 3kg of sodium carbonate, 3kg of sulfate, 10kg of copper compound, 15kg of sulfide, and 15kg of hydrosulfide;

[0028] The collector is prepared from the following components: 1 kg of oleic acid, 15 kg of 2-butyloctyl oleate, and 40 kg of petroleum cracking products.

[0029] (B) The raw ore is 100 tons of mixed flotation to get 3 tons of copper-molybdenum mixed concentrate slurry, and then 50kg inhibitor and 800g collector are added to 3 tons of copper-molybdenum mixed concentrate slurry for separation and roughing to obtain molybdenum rough concentrate 0.35 tons of pulp and 2.65 tons of copper coarse concentrate pulp, the liquid-solid mass ratio in the copper-molybdenum mixed concentrate pulp is 4:1, and the s...

Embodiment 2

[0033] Carry out copper molybdenum separation to obtain the technological process of copper concentrate and molybdenum concentrate as follows:

[0034] (A) Prepare inhibitors and collectors respectively, wherein the inhibitors are prepared from the following components: 5kg sodium carbonate, 5kg sulfate, 15kg copper compound, 20kg sulfide, 20kg hydrosulfide, and 650kg water;

[0035] The collector is prepared from the following components: 3kg of oleic acid, 25kg of 2-butyloctyl oleate, and 50kg of petroleum cracking products.

[0036] (B) 3 tons of copper-molybdenum mixed concentrate slurry is obtained from 100 tons of mixed flotation of raw ore, and 40kg of inhibitor and 1200g collector are added to 3 tons of copper-molybdenum mixed concentrate slurry for separation and roughing to obtain rough concentrate of molybdenum 0.40 tons of pulp and 2.60 tons of copper coarse concentrate pulp, the liquid-solid mass ratio in the copper-molybdenum mixed concentrate pulp is 6:1, and th...

Embodiment 3

[0041] Carry out copper molybdenum separation to obtain the technological process of copper concentrate and molybdenum concentrate as follows:

[0042] (A) Prepare inhibitors and collectors respectively, wherein the inhibitors are prepared from the following components: sodium carbonate 4kg, sulfate 4kg, copper compound 12kg, sulfide 18kg, hydrosulfide 18kg, water 560kg;

[0043]The collector is prepared from the following components: 2kg of oleic acid, 20kg of 2-butyloctyl oleate, and 45kg of petroleum cracking products.

[0044] (B) The raw ore is 100 tons of mixed flotation to get 3 tons of copper-molybdenum mixed concentrate pulp, 46kg inhibitor and 1000g collector are added to 3 tons of copper-molybdenum mixed concentrate pulp for separation and roughing to obtain molybdenum coarse concentrate pulp 0.44 tons and 2.56 tons of copper coarse concentrate slurry, the liquid-solid mass ratio in the copper-molybdenum mixed concentrate slurry is 5:1, and the separation and roughi...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The invention relates to the technical field of non-ferrous metal processing, in particular to a copper molybdenum separation flotation agent and a using method thereof. The copper molybdenum separation flotation agent comprises inhibitor for inhibiting copper mineral and collecting agent for collecting molybdenum mineral, wherein the inhibitor comprises, by weight, 3 to 5 parts of sodium carbonate, 3 to 5 parts of sulfate, 10 to 15 parts of copper compounds, 15 to 20 parts of sulfide salt, and 15 to 20 parts of hydrosulphide salt; the collecting agent comprises, by weight, 1 to 3 parts of oleic acid, 15 to 25 parts of butyl octyl oleate, and 40 to 50 parts of oil pyrolysis products. The copper molybdenum separation flotation agent and the using method thereof reduce usage amount of the agent, can achieve a certain degree of degradation in waste water if the agents are mutually matched, and thus are more environmentally friendly.

Description

technical field [0001] The invention relates to the technical field of non-ferrous metal beneficiation, in particular to a copper-molybdenum separation flotation agent and a use method thereof. Background technique [0002] Molybdenum is an element that is rarely distributed in nature. The average content in the earth's crust is about 0.001%. The United States has the most abundant molybdenum resources in the world, followed by Canada and Chile. my country's molybdenum resources are relatively rich, but now except molybdenite In addition to forming molybdenum deposits alone, they widely coexist with other sulfide beds to form polymetallic deposits, such as copper-molybdenum-sulfur deposits. [0003] For the recovery of molybdenum from copper-molybdenum ores, a lot of research work and practice have been carried out at home and abroad, most of which use the separation technology of copper-inhibiting and floating molybdenum, but the copper-inhibiting inhibitors and floating mol...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): B03D1/012B03D1/008B03D1/00B03D101/06B03D101/02
Inventor 姜良友
Owner TIBET HUATAILONG MINING DEV
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products