Preparation method of paint capable of adjusting air humidity

A technology for adjusting air and paint, applied in the direction of coating, etc., can solve the problem of limited humidity adjustment effect and so on

Inactive Publication Date: 2014-07-30
良唐福瑞至大健康科技(北京)有限公司
View PDF1 Cites 1 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

The Chinese patent application No. 200810222377.6 discloses a kind of indoor coating with humidity control function, which achieves a certain effect by adding humidity control functional materials in conventional paint, but its humidity control effect is limited, such as at 25 ℃, relative humidity Under the condition of 85%, the maximum decrease of relative humidity is 10%RH; after moisture absorption saturation, at a temperature of 25°C and a relative humidity of 35%, the coating will release moisture, and the maximum increase of relative humidity will reach 7%RH
However, there is no coating product with excellent performance in regulating air humidity.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0021] A method for preparing a paint for regulating air humidity. The paint comprises 30 parts by weight of an acrylic emulsion, 5 parts of a wetting and dispersing agent, 25 parts of hollow microspheres, 8 parts of calcareous bentonite, and 2 parts of talcum powder. Parts, 27 parts of zeolite powder, 16 parts of sepiolite, 15 parts of titanium dioxide, 12 parts of wollastonite powder, 2 parts of defoamer, 5 parts of thickener, 15 parts of starch-polyacrylonitrile graft polymer, 22 parts of water Among them, the solid content of acrylate emulsion is more than 45% and less than 60%, the minimum film-forming temperature is 1-10°C, the wetting and dispersing agent is about 10% sodium hexametaphosphate aqueous solution, and the thickener is about 2% Hydroxyethyl cellulose aqueous solution, described method comprises the steps:

[0022] 1) Add the acrylate emulsion into the water under stirring condition in the stirred tank, and stir at the speed of 600rpm for 20 minutes;

[0023...

Embodiment 2

[0028] A method for preparing a paint for regulating air humidity. The paint comprises 32 parts by weight of an acrylic emulsion, 2 parts of a wetting and dispersing agent, 35 parts of hollow microspheres, 3 parts of calcareous bentonite, and 4 parts of talcum powder. Parts, 25 parts of zeolite powder, 18 parts of sepiolite, 8 parts of titanium dioxide, 14 parts of wollastonite powder, 1 part of defoamer, 10 parts of thickener, 10 parts of starch-polyacrylonitrile graft polymer, 36 parts of water Among them, the solid content of acrylate emulsion is more than 45% and less than 60%, the minimum film-forming temperature is 1-10°C, the wetting and dispersing agent is about 10% sodium hexametaphosphate aqueous solution, and the thickener is about 2% Hydroxyethyl cellulose aqueous solution, described method comprises the steps:

[0029] 1) Add the acrylate emulsion into the water under stirring condition in the stirred tank, and stir at the speed of 800rpm for 15 minutes;

[0030]...

Embodiment 3

[0035] A method for preparing a paint for adjusting air humidity. The paint comprises 31 parts by weight of an acrylic emulsion, 3.5 parts of a wetting and dispersing agent, 30 parts of hollow microspheres, 5 parts of calcareous bentonite, and 3 parts of talcum powder. Parts, 26 parts of zeolite powder, 17 parts of sepiolite, 12 parts of titanium dioxide, 13 parts of wollastonite powder, 1.5 parts of defoamer, 8 parts of thickener, 13 parts of starch-polyacrylonitrile graft polymer, 30 parts of water Among them, the solid content of acrylate emulsion is more than 45% and less than 60%, the minimum film-forming temperature is 1-10°C, the wetting and dispersing agent is about 10% sodium hexametaphosphate aqueous solution, and the thickener is about 2% Hydroxyethyl cellulose aqueous solution, described method comprises the steps:

[0036] 1) Add the acrylate emulsion into the water under stirring condition in the stirred tank, and stir at the speed of 700rpm for 18 minutes;

[0...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
particle sizeaaaaaaaaaa
sizeaaaaaaaaaa
Login to View More

Abstract

The invention discloses a preparation method of paint capable of adjusting air humidity, the paint employs hollow bead, zeolite powder, meerschaum and starch-polyacrylonitrile graft polymers as functional materials for adjusting air humidity, and the raw materials are cooperated with other ingredients to form the paint with good effect for adjusting air humidity. The method aims at the composition characteristic of the paint for limiting the preparation step, and functional ingredients are added by batches step by step, and the prepared paint has excellent performance. According to the invention, under the condition that the temperature is 25 DEG C and the relative humidity is 85%, the relative humidity minimizing amount can reach 25-35%, the test paint has good moisture absorption effect; after saturation through moisture absorption, under the condition that the temperature is 25 DEG C and the relative humidity is 35%, the test paint is capable of releasing humidity, and the relative humidity increasing amount can reach 18-24%.

Description

technical field [0001] The invention relates to the field of chemical coatings, in particular to a preparation method of a coating for adjusting air humidity. Background technique [0002] Air relative humidity is an important parameter to measure the indoor environment, which is of great significance to human health, indoor air quality and storage of articles. [0003] Coatings are closely related to people's daily work, living and other indoor environments, and the use of functional coatings that regulate air humidity can maximize their efficacy. Air-humidity-regulating paint is a new type of functional building decoration material that has emerged in recent years, and domestic scientific researchers have begun to devote themselves to its development and research. Li Shuanglin of Beijing University of Technology prepared a ceramic air humidity regulating coating with organic resin as the functional material for regulating air humidity (Li Shuanglin, Wu Yuting, Ma Chongfan...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Applications(China)
IPC IPC(8): C09D133/04C09D151/02C09D7/12C09D5/00
Inventor 朱小英
Owner 良唐福瑞至大健康科技(北京)有限公司