A kind of imitation granite paint, colorful technology, applied in the field of building decoration and decoration materials, can solve the problems of inability to guarantee the stability of paint particles, difficult industrial production, etc., to solve water resistance and product transportation, good granulation effect, and solve environmental pollution problem effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0036] (1) Preparation of color particle components (monochrome): Weigh 40 parts of 661B silicone acrylic emulsion, 30 parts of deionized water, 0.6 parts of ammonium salt dispersant, 0.5 part of wetting agent, 0.2 part of defoamer, and 0.1 part of preservative Parts, 15 parts of powder, disperse at high speed (1500r / min-1800r / min) until the surface is shiny, add 2 parts of modified bentonite, disperse at medium and high speed (1000r / min-1200r / min) for 15 minutes, and disperse at medium speed (500r / min) min-800r / min) under stirring, add 3 parts of film-forming aids, 4 parts of ethylene glycol, and AMP-952 parts into the water, stir for 5min-10min, add pigments and fillers at a uniform speed, high speed (1200r / min-1500r / min ) after dispersing for 20 minutes, use a grinder to grind to a fineness below 50 μm, add the measured 661B silicon acrylic emulsion, stir at a medium speed (500r / min-800r / min) for 20 minutes, add a thickener to adjust the viscosity to 120-130μ to obtain Sing...
Embodiment 2
[0042] (1) Preparation of color particle components (single color): weigh 30 parts of 661B silicone acrylic emulsion, 40 parts of deionized water, 0.6 parts of ammonium salt dispersant, 0.5 part of wetting agent, 0.2 part of defoamer, and 0.1 part of preservative Parts, 15 parts of powder, disperse at high speed (1500r / min-1800r / min) until the surface is shiny, add 2 parts of modified bentonite, disperse at medium and high speed (1000r / min-1200r / min) for 15 minutes, and disperse at medium speed (500r / min) / min-800r / min) under stirring, add 3 parts of film-forming aids, 4 parts of ethylene glycol, and AMP-952 parts into the water, stir for 5min-10min, add pigments and fillers at a uniform speed, high speed (1200r / min-1500r / min) After dispersing for 20 minutes, use a grinder to grind to a fineness below 50 μm, add the measured 661B silicone acrylic emulsion, stir at a medium speed (500r / min-800r / min) for 20 minutes, add a thickener to adjust the viscosity to 120-130μm Obtain mo...
Embodiment 3
[0048] (1) Preparation of color particle components (single color): Weigh 45 parts of HRS-180 styrene-acrylic emulsion, 25 parts of deionized water, 0.6 part of ammonium salt dispersant, 0.5 part of wetting agent, 0.2 part of defoamer, anti-corrosion 0.1 part of agent, 15 parts of powder, disperse at high speed (1500r / min-1800r / min) until the surface is shiny, add 2 parts of modified bentonite, disperse at medium and high speed (1000r / min-1200r / min) for 15 minutes, and disperse at medium speed ( 500r / min-800r / min) under stirring, add 3 parts of film-forming aids, 4 parts of ethylene glycol, AMP-952 parts into the water, stir for 5min-10min, add pigments and fillers at a uniform speed, high speed (1200r / min-1500r / min) After dispersing for 20 minutes, use a grinder to grind to a fineness below 50 μm, add the measured HRS-180 styrene-acrylic emulsion, stir at a medium speed (500r / min-800r / min) for 20 minutes, add a thickener to adjust the viscosity to 120-130μ to obtain monochro...