Natural polymer fluid loss reducer for drilling fluid and its preparation method and application
A technology of natural polymer and fluid loss control agent, which is applied in the field of natural polymer fluid loss control agent and its preparation, can solve environmental pollution and other problems, and achieve the effects of no biological toxicity, excellent temperature resistance, and strong fluid loss control ability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0020] Get 20 parts of water by weight, under stirring respectively 80 parts of konjac gum, 15 parts of soda ash, 5 parts of urea, 6 parts of glycerin, 35 parts of 95% ethanol are joined in the kneader, pass into steam in the kneader jacket, The temperature was kept at 80°C for 3 hours. After completion of the reaction, pour cold water into the jacket, discharge the material after cooling, dry at 110° C. for 4.5 hours and pulverize to obtain the natural polymer fluid loss reducer for drilling fluid of this embodiment.
Embodiment 2
[0022] Get 15 parts of water by weight ratio, under stirring, respectively 75 parts of konjac gum, 17 parts of soda ash, 6 parts of urea, 7 parts of glycerin, 40 parts of 95% ethanol are joined in the kneader, pass into steam in the kneader jacket, The temperature was maintained at 85°C for 4 hours. After completion of the reaction, pour cold water into the jacket, discharge the material after cooling, dry at 100° C. for 6 hours, and pulverize to obtain the natural polymer fluid loss reducer for drilling fluid of this embodiment.
Embodiment 3
[0024] Get 25 parts of water by weight, under stirring respectively 90 parts of konjac gum, 20 parts of soda ash, 4 parts of urea, 5 parts of glycerin, 30 parts of 95% ethanol are joined in the kneader, pass into steam in the kneader jacket, The temperature was maintained at 90°C for 3.5 hours. After completion of the reaction, pour cold water into the jacket, discharge the material after cooling, dry at 120° C. for 4 hours and pulverize to obtain the natural polymer fluid loss reducer for drilling fluid of this embodiment.
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More 