Embodiment 1
[0025] The raw material in this example is the white tailings in the process of producing quartz sand from vein quartz ore produced by Tangshan Jinxin Shida Silicon Industry Co., Ltd. The specific production process is as follows:
[0026] 1. Rinse the quartz tailings with clean water first, then centrifuge and dehydrate, and detect the impurities in it: Al 2 o 3 : 0.16%, Fe 2 o 3 : 0.053%, K 2 O: 0.02%, Na 2 O: 0.01%; Moisture: 5.6%
[0027] 2. Surface cleaning and impurity removal
[0028] Put the quartz tailings in step 1 into the reaction kettle, first turn on the acid mist absorption tower system, so that the whole reaction system is in a state of slight negative pressure, then turn on the jacket cooling water of the kettle and the condenser cooling water, and then turn on the acid mist absorption tower system. Pump, use a frequency converter to control the amount of hydrofluoric acid sent into the kettle. The concentration of hydrofluoric acid is 10% (depending on ...
Embodiment 2
[0033] The raw material in this example is the yellow tailing sand in the process of producing quartz sand from sedimentary quartzite produced by a silica sand Co., Ltd. in Yishui, Linyi. The specific production process is as follows:
[0034] 1. Since the tailings are long-term stacked tailings, the quartz tailings are beaten first, rinsed with clean water, and then centrifugally dehydrated to detect impurities: Al 2 o 3 : 0.94%, Fe 2 o 3 : 0.15%, K 2 O: 0.02%, Na 2 O: 0.36%; Moisture: 6.3%
[0035] 2. Surface cleaning and impurity removal
[0036] Put the quartz tailings in step 1 into the reaction kettle, first turn on the acid mist absorption tower system, so that the whole reaction system is in a state of slight negative pressure, then turn on the jacket cooling water of the kettle and the condenser cooling water, and then turn on the acid mist absorption tower system. Pump, use a frequency converter to control the amount of hydrofluoric acid sent into the kettle. T...
Embodiment 3
[0041] The raw material in this example is light white tailing sand in the process of producing quartz sand from sedimentary quartzite produced by a silica sand technology Co., Ltd. in Fengyang, Anhui. The specific production process is as follows:
[0042] 1. Since the sand powder is dry sand powder, the impurities in it are directly detected: Al 2 o 3 : 2.44%, Fe 2 o 3 : 0.058%, K 2 O: 0.13%, Na 2 O: 0.01%; Moisture: 4.3%.
[0043] 2. Surface cleaning and impurity removal
[0044] Put the quartz tailings in step 1 into the reaction kettle, first turn on the acid mist absorption tower system, so that the whole reaction system is in a state of slight negative pressure, then turn on the jacket cooling water of the kettle and the condenser cooling water, and then turn on the acid mist absorption tower system. Pump, use a frequency converter to control the amount of fluosilicic acid sent into the kettle, the concentration of fluosilicic acid is 30% (depending on the situati...