Preparation method of aluminum carried pulverized fuel ash applied to recycling of phosphorus resources in waste water
A technology for fly ash and phosphorus resources, which is applied in chemical instruments and methods, adsorption water/sewage treatment, other chemical processes, etc., to achieve the effects of simple preparation method, realization of regeneration, and low energy consumption
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0026] The preparation method of aluminum-loaded fly ash: first, put the fly ash in a container containing 0.05mol·L -1 Soak in the container of aluminum sulfate solution for 1 day and night; then, pour out the aluminum sulfate solution in the container, and wash the fly ash with water, after cleaning, pour off the water, then add water to the container where the fly ash Higher than fly ash; Afterwards, drip sodium hydroxide solution in water under stirring action, the pH value of water is slowly raised to 7.5-8.0, and the time of controlling whole sodium hydroxide solution dripping process is 0.5 hour; Finally, Separate the fly ash from the water and let it dry.
Embodiment 2
[0028] The preparation method of aluminum-loaded fly ash: first, put the fly ash in a container containing 0.6mol·L -1 Then, pour out the aluminum nitrate solution in the container, and wash the fly ash with water. After cleaning, pour off the water, then add water to the container where the fly ash is located, and make the water surface Higher than fly ash; Afterwards, drip potassium hydroxide solution in water under stirring action, make the pH value of water slowly rise to 7.5-8.0, control the time of whole potassium hydroxide solution dripping process to be 1.5 hours; Finally, Separate the fly ash from the water and put it into a muffle furnace for high temperature treatment at 300°C for 16 hours.
Embodiment 3
[0030] The preparation method of aluminum-loaded fly ash: first, the fly ash was mixed in 0.1mol·L -1 Soak in dilute sulfuric acid for 3 days and nights; then, put the fly ash in a container containing 0.3mol·L -1 Then, pour out the aluminum chloride solution in the container, and wash the fly ash with water. After cleaning, pour off the water, add water to the container where the fly ash is located, and Make the water surface higher than the fly ash; after that, add potassium hydroxide solution dropwise to the water under the action of stirring, so that the pH value of the water is slowly raised to 7.5-8.0, and the time for controlling the whole process of adding potassium hydroxide solution is 1 hour; Finally, the fly ash is separated from the water and allowed to dry.
PUM
| Property | Measurement | Unit |
|---|---|---|
| particle size (mesh) | aaaaa | aaaaa |
Abstract