Anti-corrosion paint and preparation method thereof
An anti-corrosion coating and modification technology, used in anti-corrosion coatings, polyurea/polyurethane coatings, coatings, etc., can solve the problems of coating foaming and wrinkling, narrow application range, easy to cause cancer, etc., and achieve corrosion resistance and aging resistance. Good, good application prospects, long service life
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0019] An anti-corrosion coating, comprising the following components by weight: 60 parts of epoxy-terminated modified polyurethane resin, 35 parts of acrylic resin, 3 parts of graphene, 5 parts of povidone-iodine, 3 parts of nano-zinc sulfide, nano-concave-convex 5 parts of stick clay, 3 parts of talc, 2 parts of hexabromocyclododecane, 1 part of isooctyl tin dimethyl dimercaptoacetate, 5 parts of gum arabic, 3 parts of dibutyl phthalate, ethyl acetate 6 parts, 12 parts of tributyl phosphate, 37 parts of acetone, 4 parts of leveling agent.
[0020] In this example, 0.2 parts of pigment are also included. The leveling agent is an acrylic leveling agent.
[0021] The preparation method of above-mentioned anticorrosion paint, described method comprises the steps:
[0022] Step 1: Add ethyl acetate and acetone to a high-speed mixer, then add nano-zinc sulfide, nano-attapulgite, talcum powder, and graphene, and stir at a speed of 1000 rpm for 15 minutes to obtain component I;
...
Embodiment 2
[0026] An anti-corrosion paint, comprising the following components by weight: 69 parts of epoxy-terminated polyurethane resin, 41 parts of acrylic resin, 6 parts of graphene, 7 parts of povidone-iodine, 4.5 parts of nano-zinc sulfide, nano-concave-convex 6 parts of stick clay, 4 parts of talc, 3.5 parts of hexabromocyclododecane, 3 parts of isooctyl tin dimethyldithioglycolate, 7 parts of gum arabic, 5 parts of dibutyl phthalate, ethyl acetate 10 parts, 15 parts of tributyl phosphate, 41 parts of acetone, 6 parts of leveling agent.
[0027] In this example, 2.5 parts of pigment are also included. The leveling agent is a silicone leveling agent leveling agent.
[0028] The preparation method of above-mentioned anticorrosion paint, described method comprises the steps:
[0029] Step 1: Add ethyl acetate and acetone to a high-speed mixer, then add nano-zinc sulfide, nano-attapulgite, talcum powder, and graphene, and stir for 22 minutes at a speed of 1400 rpm to obtain componen...
Embodiment 3
[0033] An anti-corrosion coating, comprising the following components by weight: 78 parts of epoxy-terminated polyurethane resin, 46 parts of acrylic resin, 8 parts of graphene, 9 parts of povidone-iodine, 6 parts of nano-zinc sulfide, nano-concave-convex 8 parts of stick clay, 6 parts of talc, 5 parts of hexabromocyclododecane, 5 parts of isooctyl tin dimethyl dimercaptoacetate, 10 parts of gum arabic, 7 parts of dibutyl phthalate, ethyl acetate 13 parts, 18 parts of tributyl phosphate, 45 parts of acetone, 9 parts of leveling agent.
[0034] In this example, 5 parts of pigment are also included. The leveling agent is a fluorocarbon leveling agent.
[0035] The preparation method of above-mentioned anticorrosion paint, described method comprises the steps:
[0036] Step 1: Add ethyl acetate and acetone to a high-speed mixer, then add nano-zinc sulfide, nano-attapulgite, talcum powder, and graphene, and stir at a speed of 1800 rpm for 30 minutes to obtain component I;
[00...