Embodiment 1
[0030] A kind of deodorant antibacterial leather production technology, its steps are:
[0031] Step 1, weighing: Weigh the raw material wet blue hide;
[0032] Step 2, degreasing: Put the wet blue hide into the drum with water at about 45°C and rotate, add degreasing agent and formic acid, rotate for 60 minutes, and then wash with water; wash;
[0033] Step 3, neutralization: at room temperature, put the wet blue leather into the drum, add water, then add ammonium bicarbonate and baking soda, rotate for 90 minutes, and then wash with water; wash;
[0034] Step 4, dyeing: at room temperature, put the wet blue leather into an anhydrous drum, add 2% ammonia water, rotate for 10 minutes, then add anionic dyes and rotate for 70 minutes;
[0035] Step 5, fatliquing: add water at 60°C to the drum, add anionic fatliquoring agent, and rotate for 70 minutes; the temperature inside the drum is 55°C;
[0036] Step 6, solid acid: add 0.5% formic acid, rotate for 15 minutes, then add 1% ...
Embodiment 2
[0048] A kind of deodorant antibacterial leather production technology, its steps are:
[0049] Step 1, weighing: Weigh the raw material wet blue hide;
[0050] Step 2, degreasing: Put the wet blue hide into the drum with water at about 45°C and rotate, add degreasing agent and formic acid, rotate for 60 minutes, and then wash with water; wash.
[0051] Step 3, neutralization: at room temperature, put the wet blue hide into the drum, add water, then add ammonium bicarbonate and baking soda, rotate for 90 minutes, and then wash with water; wash.
[0052] Step 4, dyeing: under normal temperature conditions, put the wet blue leather into an anhydrous drum, add 2% ammonia water, rotate for 10 minutes, then add anionic dyes and rotate for 70 minutes;
[0053] Step 5, fatliquing: add water at 60°C to the drum, add anionic fatliquoring agent, and rotate for 70 minutes; the temperature inside the drum is 55°C;
[0054] Step 6, solid acid: add 0.5% formic acid, rotate for 15 minutes,...
Embodiment 3
[0066] A kind of deodorant antibacterial leather production technology, its steps are:
[0067] Step 1, weighing: Weigh the raw material wet blue hide;
[0068] Step 2, degreasing: put in water for rotation at a temperature of 45°C, add degreasing agent and formic acid, rotate for 60 minutes, and then wash with water;
[0069] Step 3, neutralization: put the wet blue skin into water at room temperature, then add ammonium bicarbonate and baking soda, rotate for 90 minutes, and then clear the water;
[0070] Step 4, dyeing: at room temperature, add 2% ammonia water, rotate for 10 minutes, then add anionic dye and rotate for 70 minutes;
[0071] Step 5, fatliquor: add anionic fatliquor to water at 55°C, and rotate for 70 minutes;
[0072] Step 6, solid acid: add 0.5% formic acid, rotate for 15 minutes, then add 1% formic acid, rotate for 15 minutes, finally add 1% formic acid, rotate for 30 minutes, wash with water after stopping;
[0073] Step 7, deodorant and antibacterial: ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com