Smooth brightener for treating wool or wool-containing fabrics and preparation method of smooth brightener
A technology of brightening agent and wool, which is applied in fiber processing, animal fiber, textiles and papermaking, etc., can solve the problems of lower grade of fabric products, not bright enough fabric color, poor soft hand feeling of fabric, etc., achieves reduced dosage, convenient preparation, Excellent washing resistance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0035] A method for preparing a smooth brightening agent for processing wool or wool-containing fabrics, comprising the following steps:
[0036] (1) Weighing: Inspect various raw materials according to the requirements, and weigh them according to the proportion of the formula for later use;
[0037](2) Add the deionized book into the reaction kettle equipped with a stirring device, adjust the temperature of the reaction kettle to 45°C, and after the temperature is stable, add D4 octamethylcyclotetrasiloxane with a weight percentage of 23% In the reaction kettle, turn on the stirring device, the stirring device rotates at 100 rpm, and the stirring time is 30 minutes, until the stirring is uniform, and during the stirring process, the temperature of the reaction kettle is raised to 95°C;
[0038] (3) After the stirring is completed, continue to control the temperature of the reactor at 95°C, add 5% polyoxyethylene ether 8810 and 6% polyether into the reactor in turn, turn on t...
Embodiment 2
[0044] A method for preparing a smooth brightening agent for processing wool or wool-containing fabrics, comprising the following steps:
[0045] (1) Weighing: Inspect various raw materials according to the requirements, and weigh them according to the proportion of the formula for later use;
[0046] (2) Put the deionized book into the reaction kettle equipped with a stirring device, adjust the temperature of the reaction kettle to 47°C, after the temperature is stable, add D4 octamethylcyclotetrasiloxane with a weight percentage of 25% Into the reaction kettle, turn on the stirring device, the stirring device speed is 150rpm, the stirring time is 40min, until the stirring is uniform, the temperature of the reaction kettle is raised to 95°C during the stirring process;
[0047] (3) After the stirring is completed, continue to control the temperature of the reactor at 95°C, add 8.5% polyoxyethylene ether 8810 and 8% polyether into the reactor in turn, turn on the stirring devi...
Embodiment 3
[0053] (1) Weighing: Inspect various raw materials according to the requirements, and weigh them according to the proportion of the formula for later use;
[0054] (2) Put the deionized book into the reaction kettle equipped with a stirring device, adjust the temperature of the reaction kettle to 50°C, after the temperature is stable, add D4 octamethylcyclotetrasiloxane with a weight percentage of 26% Into the reactor, turn on the stirring device, the stirring device rotates at 200rpm, and the stirring time is 50min, until the stirring is even, during the stirring process, the temperature of the reactor is raised to 95°C;
[0055] (3) After the stirring is completed, continue to control the temperature of the reactor at 95°C, add 10% polyoxyethylene ether 8810 and 9% polyether into the reactor in turn, turn on the stirring device, and the stirring device rotates 200rpm, stirring time is 30min, until the stirring is uniform;
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com