A technology of warm mixing agent and asphalt, which is applied in the direction of building insulation materials, building components, climate change adaptation, etc., can solve the problems of reducing the high temperature stability of asphalt, and achieve the effect of improving fluidity, fluidity, and temperature resistance

Inactive Publication Date: 2017-10-20
常州市雄图纺织有限公司
View PDF5 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0005] The technical problem to be solved by the present invention: Aiming at the problem that the current asphalt warm mix agent reduces the viscosity of asphalt at 60°C, that is, reduces the high temperature stability of asphalt, a kind of asphalt warm mix agent and its preparation method are provided

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Asphalt warm-mixing agent and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

preparation example Construction

[0019] Preparation of additives: Put strontium carbonate, nano-titanium dioxide and polydimethylsilane into a mill at a mass ratio of 4:3:5, mill at 800r / min for 30-35min, collect the milled mixture, and that’s it.

[0020] Preparation of mixed acid: Mix sulfamic acid, 3-chloropropionic acid and oxalic acid in a mass ratio of 2:3:2.

[0021] The asphalt warm mix agent of the present invention comprises the following raw materials in parts by weight: 70 to 90 parts of water, 30 to 50 parts of sucrose fatty acid ester, 20 to 25 parts of alkyl glycoside, 13 to 16 parts of mixed acid, 6 to 8 parts Additives, 2-5 parts of hydroxypropyl methylcellulose.

[0022] The preparation method of asphalt warm mix agent of the present invention is characterized in that, comprises following preparation steps:

[0023] (1) Take raw materials according to the ratio of parts by weight;

[0024] (2) Put water, sucrose fatty acid ester and alkyl glycoside into the reactor, use 2.1mol / L sodium hyd...

example 1

[0028] Preparation of additives: Put strontium carbonate, nano-titanium dioxide and polydimethylsilane into a mill at a mass ratio of 4:3:5, mill at 800r / min for 35min, and collect the milled mixture.

[0029] Preparation of mixed acid: Mix sulfamic acid, 3-chloropropionic acid and oxalic acid in a mass ratio of 2:3:2.

[0030] The asphalt warm mix agent of the present invention comprises the following raw materials in parts by weight: 70 parts of water, 30 parts of sucrose fatty acid esters, 20 parts of alkyl glucosides, 13 parts of mixed acids, 6 parts of additives, 2 parts of hydroxypropyl methyl cellulose.

[0031] The preparation method of asphalt warm mix agent of the present invention is characterized in that, comprises following preparation steps:

[0032] (1) Take raw materials according to the ratio of parts by weight;

[0033] (2) Put water, sucrose fatty acid ester and alkyl glucoside into the reactor, use 2.1mol / L sodium hydroxide solution to adjust the pH to 8....

example 2

[0037] Preparation of additives: Put strontium carbonate, nano-titanium dioxide and polydimethylsilane into a mill at a mass ratio of 4:3:5, mill at 800r / min for 35min, and collect the milled mixture.

[0038] Preparation of mixed acid: Mix sulfamic acid, 3-chloropropionic acid and oxalic acid in a mass ratio of 2:3:2.

[0039] The asphalt warm mix agent of the present invention comprises the following raw materials in parts by weight: 90 parts of water, 50 parts of sucrose fatty acid esters, 25 parts of alkyl glucosides, 16 parts of mixed acids, 8 parts of additives, 5 parts of hydroxypropyl methyl cellulose.

[0040] The preparation method of asphalt warm mix agent of the present invention is characterized in that, comprises following preparation steps:

[0041] (1) Take raw materials according to the ratio of parts by weight;

[0042] (2) Put water, sucrose fatty acid ester and alkyl glucoside into the reactor, use 2.1mol / L sodium hydroxide solution to adjust the pH to 8....

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention relates to an asphalt warm-mixing agent and a preparation method thereof, which belongs to the technical field of pavement laying materials. The preparation method comprises the following steps: mixing and grinding strontium carbonate, nano titanium dioxide and polydimethylsilane, thus obtaining an additive, mixing sulfamic acid, 3-chloropropionic acid and ethanedioic acid to obtain a mixed acid, then placing water, sucrose fatty acid ester and alkyl glycoside into a reactor, adjusting the pH by utilizing a sodium hydroxide solution, stirring, standing, cooling, adding the mixed acid and hydroxypropyl methyl cellulose, increasing the pressure under the protection of nitrogen, stirring, cooling to room temperature, discharging materials, collecting the discharged materials, stirring and mixing the discharged materials and absolute ethyl alcohol, standing, distilling, collecting residues, stirring and mixing the residues and additives, and collecting a stirred mixture, thus obtaining the asphalt warm-mixing agent. The asphalt mixing agent prepared by the invention can effectively improve the viscosity of asphalt at 60 DEG C and is relatively good in high-temperature stability.

Description

technical field [0001] The invention relates to an asphalt warm mix agent and a preparation method thereof, specifically belonging to the technical field of road paving materials. Background technique [0002] Warm mix asphalt technology is a kind of asphalt mixing whose mixing temperature is between hot mix asphalt technology (150-180°C) and cold mix asphalt technology (10-40°C), and its performance reaches (or is close to) hot mix asphalt mixture. Energy-saving new technology. Usually, the most common implementation method of warm mix technology is to add warm mix agent. Compared with standard hot mix asphalt technology, the temperature of warm mix asphalt technology can be reduced by 20-30°C. Warm mix asphalt technology has many advantages: firstly, the production and construction temperature of asphalt mixture can be reduced, which can save more than 20% of energy consumption; at the same time, the storage temperature of asphalt mixture is lowered, and the fluidity at l...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Applications(China)
IPC IPC(8): C08L95/00C08L83/04C08L1/28C08K13/02C08K5/1545C08K3/26C08K3/22C08K5/42
CPCC08K2003/2241C08K2003/265C08L95/005C08L2201/08C08L2205/03C08L83/04C08L1/284C08K13/02C08K5/1545C08K3/26C08K3/22C08K5/42Y02A30/30
Inventor 李兴才薛焱璟王磊
Owner 常州市雄图纺织有限公司