Preparation method of refine cotton
A technology for refining cotton and cotton pulp, applied in textile and papermaking, pulp bleaching, fiber raw material processing, etc., can solve the problems of high maturity, product whiteness not meeting demand, difficult process control, etc., to achieve low water consumption Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0021] The present invention is carried out according to the following steps:
[0022] 1) material selection, cotton opening, cooking: take cotton linters as raw material and add cooking liquid after cotton opening and impurity removal, and cook at 120 ° C; wherein, in the cooking liquid, KOH content is 18g / l, and the weight percent of emulsifier is 0.1%, the emulsifier is sodium alkyl benzene sulfonate; the material-to-liquid weight ratio is 1:5 during cooking;
[0023] 2) Pre-bleaching: the absorbent cotton after cooking is washed with water to obtain cotton pulp, and then H2O2 and acetone peroxide mixed solution are added for pre-bleaching;
[0024] 3) Acidification: the cotton pulp after pre-bleaching is acidified for 2h under the condition of pH 6;
[0025] 4) Bleaching: add a mixed solution of H2O2 and chlorine dioxide between 30-50 degrees, the amount of the mixed solution is 4% of the quality of the refined cotton, and it is made by stirring for 12 minutes.
[0026] ...
Embodiment 2
[0033] The present invention is carried out according to the following steps:
[0034] 1) material selection, cotton opening, cooking: take cotton linters as raw material and add cooking liquid after cotton opening and impurity removal, and cook at 100 ° C; wherein, in the cooking liquid, KOH content is 16g / l, and the weight percent of emulsifier is 0.1%, the emulsifier is sodium alkyl benzene sulfonate; the material-to-liquid weight ratio is 1:6 during cooking;
[0035] 2) Pre-bleaching: the absorbent cotton after cooking is washed with water to obtain cotton pulp, and then H2O2 and acetone peroxide mixed solution are added for pre-bleaching;
[0036] 3) Acidification: the cotton pulp after pre-bleaching is acidified under the condition of pH 4 for 1-2h;
[0037] 4) Bleaching: add a mixed solution of H2O2 and chlorine dioxide between 45 degrees, the amount of the mixed solution is 5% of the quality of the refined cotton, and it is made by stirring for 15 minutes.
[0038] I...
Embodiment 3
[0045] The present invention is carried out according to the following steps:
[0046] 1) material selection, cotton opening, cooking: take cotton linters as raw material and add cooking liquid after cotton opening and impurity removal, and cook at 115 DEG C; wherein, in the cooking liquid, KOH content is 15g / l, and the weight percent of emulsifier is 0.25%, the emulsifier is sodium alkyl benzene sulfonate; the material-liquid weight ratio is 1:5 during cooking;
[0047] 2) Pre-bleaching: the absorbent cotton after cooking is washed with water to obtain cotton pulp, and then H2O2 and acetone peroxide mixed solution are added for pre-bleaching;
[0048] 3) Acidification: the cotton pulp after pre-bleaching is acidified under the condition of pH 6 for 1-2h;
[0049] 4) Bleaching: add a mixed solution of H2O2 and chlorine dioxide between 40 degrees, the amount of the mixed solution is 4% of the quality of the refined cotton, and it is made by stirring for 10 minutes.
[0050] I...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com