Embodiment 1
[0029] A plastomer-modified asphalt waterproof coiled material, which sequentially comprises an isolation layer, a plastomer-modified asphalt coating, a base layer, a plastomer-modified asphalt coating, and an isolation layer.
[0030] Wherein, the isolation layer is prepared, in parts by mass, the consumption of the EPDM rubber is 40 parts, the consumption of the polyisobutylene rubber is 70 parts, and the consumption of the ultrafine calcium carbonate is 15 parts, the The consumption of the antioxidant is 1 part, the consumption of the accelerator is 1 part, and the consumption of the reinforcing agent is 1 part.
[0031] Wherein, the plastomer modified asphalt coating is prepared, in parts by mass, the consumption of the 100# petroleum asphalt is 100 parts, the consumption of the modified rubber powder is 15 parts, and the consumption of the atactic polypropylene is 11 parts, the consumption of the coupling agent is 4 parts, and the consumption of the filler is 24 parts.
Embodiment 2
[0033] A plastomer-modified asphalt waterproof coiled material, which sequentially comprises an isolation layer, a plastomer-modified asphalt coating, a base layer, a plastomer-modified asphalt coating, and an isolation layer.
[0034] Wherein, to prepare the isolation layer, in parts by mass, the consumption of the EPDM rubber is 30 parts, the consumption of the polyisobutylene rubber is 80 parts, and the consumption of the ultrafine calcium carbonate is 10 parts, the The consumption of the antioxidant is 2 parts, the consumption of the accelerator is 0.5 parts, and the consumption of the reinforcing agent is 1.5 parts.
[0035] Wherein, the plastomer modified asphalt coating is prepared, in parts by mass, the consumption of the 100# petroleum asphalt is 90 parts, the consumption of the modified rubber powder is 20 parts, and the consumption of the atactic polypropylene is 10 parts, the consumption of described coupling agent is 5 parts, and the consumption of described fille...
Embodiment 3
[0037] A plastomer-modified bitumen waterproof coiled material, which sequentially comprises an isolation layer, a plastomer-modified asphalt coating, a base layer, a plastomer-modified asphalt coating, and an isolation layer.
[0038] Wherein, to prepare the isolation layer, in parts by mass, the consumption of the EPDM rubber is 50 parts, the consumption of the polyisobutylene rubber is 60 parts, and the consumption of the ultrafine calcium carbonate is 20 parts, the The consumption of the antioxidant is 1 part, the consumption of the accelerator is 1.5 parts, and the consumption of the reinforcing agent is 0.5 parts.
[0039] Wherein, the plastomer modified asphalt coating is prepared, in parts by mass, the consumption of the 100# petroleum asphalt is 100 parts, the consumption of the modified rubber powder is 10 parts, and the consumption of the atactic polypropylene is 20 parts, the consumption of the coupling agent is 3 parts, and the consumption of the filler is 30 part...