Unlock instant, AI-driven research and patent intelligence for your innovation.

Preparation process of texture coating suitable for external wall insulation matching

A textured coating and preparation process technology, applied in coatings, inorganic chemistry, titanium compounds, etc., can solve the problems of destroying the aesthetics of the finish, reducing the hardness of the coating surface, and being prone to scratches, ensuring storage stability, increasing Large interaction force, the effect of improving the appearance and decoration effect

Inactive Publication Date: 2020-12-04
安徽喜宝高分子材料有限公司
View PDF7 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

For example, Chinese patent CN2006100447294 discloses an inorganic anti-cracking floor coating, which provides that adding anti-cracking chemical fibers in the coating can effectively prevent the cracking of the surface mortar, but in the coating matrix, the added anti-cracking chemical fibers are easily separated. Cross-linking and agglomeration occur, forming sedimentation, which makes the storage stability of the paint poor; another example is Chinese patent CN2011104257800 which discloses an elastic texture paint, which uses a special pure acrylic emulsion as the base material to prepare an elastic emulsion, which can effectively bridge the gap by improving the flexibility of the paint. Even the cracks of the wall, so as to achieve the technical effect of anti-cracking, but the improvement of the flexibility of the paint makes the surface hardness of the paint lower, and scratches are prone to appear under the action of external wind and sand, which destroys the aesthetics of the finish

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0018] A preparation process for a textured coating suitable for external wall insulation, the specific process method is as follows:

[0019] 1) According to the volume ratio of 1:6:15, weigh the titanium chloride solution with a mass concentration of 16%, absolute ethanol and distilled water, stir them evenly and transfer them into a stainless steel autoclave lined with polytetrafluoroethylene. Heating at a constant temperature for 13 hours, filtering the obtained product, rinsing with deionized water and absolute ethanol respectively, and drying to obtain titanium dioxide fibers;

[0020] 2) According to the mass-volume ratio of 4g:7g:250mL, weigh zinc acetate dihydrate and polyvinylpyrrolidone, add them to deionized water in turn, stir at room temperature at 100r / min for 30min to obtain a transparent solution, and then according to the mass-volume ratio: 4:100g / mL, add sodium stannate trihydrate into deionized water, stir evenly, and slowly add it dropwise to the above tra...

Embodiment 2

[0026] A preparation process for a textured coating suitable for external wall insulation, the specific process method is as follows:

[0027] 1) According to the volume ratio of 1:7:18, weigh the titanium chloride solution with a mass concentration of 18%, absolute ethanol and distilled water, stir them evenly, and transfer them into a stainless steel autoclave lined with polytetrafluoroethylene, at 155°C Heating at a constant temperature for 12 hours, filtering the obtained product, rinsing with deionized water and absolute ethanol respectively, and drying to obtain titanium dioxide fibers;

[0028] 2) According to the mass-volume ratio of 4.2:7g:280mL, weigh zinc acetate dihydrate and polyvinylpyrrolidone, add them to deionized water in turn, stir at room temperature at 130r / min for 35min to obtain a transparent solution, and then according to the mass-volume ratio 4.3: 100g / mL, add sodium stannate trihydrate into deionized water, stir evenly, according to the volume ratio ...

Embodiment 3

[0034] A preparation process for a textured coating suitable for external wall insulation, the specific process method is as follows:

[0035] 1) According to the volume ratio of 1:8:20, weigh titanium chloride solution with a mass concentration of 20%, absolute ethanol and distilled water, stir evenly, transfer to a stainless steel autoclave lined with polytetrafluoroethylene, at 160°C Heating at a constant temperature for 10 hours, filtering the obtained product, rinsing with deionized water and absolute ethanol respectively, and drying to obtain titanium dioxide fibers;

[0036] 2) According to the mass volume ratio of 4.5g:7g:300mL, weigh zinc acetate dihydrate and polyvinylpyrrolidone, add them to deionized water in turn, stir at 140r / min at room temperature for 40min to obtain a transparent solution, and then 4.5:100g / mL, add sodium stannate trihydrate into deionized water, stir evenly, according to the volume ratio of 1:3, slowly drop into the above transparent solution...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
Particle sizeaaaaaaaaaa
Particle sizeaaaaaaaaaa
Particle sizeaaaaaaaaaa
Login to View More

Abstract

The invention discloses a preparation process of a texture coating suitable for external wall insulation matching, and relates to the technical field of coating processing, and the preparation processcomprises the following steps: 1) preparing titanium dioxide fibers by adopting a titanium chloride solution, absolute ethyl alcohol and distilled water; 2) preparing nano-scale carboxyl zinc stannate by taking zinc acetate dihydrate sodium stannate trihydrate as a raw material; 3) dispersing nanoscale zinc carboxystannate in the chitosan solution, and adding titanium dioxide fibers to prepare titanium dioxide composite fibers; 4) pretreating the titanium dioxide composite fiber; and 5) uniformly mixing the raw materials under a stirring condition to obtain the required texture coating. The pretreated titanium dioxide composite fibers are added into a conventional texture coating matrix, an intermolecular photoaddition reaction occurs under illumination, a cross-linked network is formed,the intermolecular interaction force in the coating matrix can be increased, the coating is not prone to cracking, the problem of tiny cracks caused by wall cracking can be solved, the service life ofthe coating is prolonged, and the appearance decoration effect is improved.

Description

technical field [0001] The invention belongs to the technical field of paint processing, and in particular relates to a preparation process of texture paint suitable for external wall heat preservation. Background technique [0002] With its infinitely varied three-dimensional textures and multiple choices of individual collocations, textured paints show a unique spatial perspective, rich and vivid, refreshing, and satisfy the overall decoration style with individual creations, making textured paints show themselves in the decoration unique style. This new type of art paint brings the smooth era of wall paint into a new era of natural environmentally friendly concave-convex paint, which can replace wallpaper, and is more environmentally friendly, economical and personalized. Texture paint has no radiation, light weight, and realistic effects. Through different construction techniques, techniques and techniques, it can create endless special decorative effects. This is a ne...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
IPC IPC(8): C09D133/00C09D7/62D06M11/46D06M15/03D06M15/233D06M11/72C01G23/053
CPCC01G23/0536C01P2004/10C09D133/00C09D7/62C09D7/70D06M11/46D06M11/72D06M15/03D06M15/233C08L1/28C08K13/06C08K9/08C08K9/02C08K7/08
Inventor 李振飞
Owner 安徽喜宝高分子材料有限公司