Bearing and heat dissipation integrated X-core corrugated wall square hole honeycomb and preparation method thereof
A corrugated wall and honeycomb technology, which is applied in the field of bearing and heat dissipation integrated X-core corrugated wall square hole honeycomb and its preparation, can solve the problem of uneven flow distribution and other issues
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0052] Embodiment 1: as figure 1 Preparation of sandwich panels shown (304 stainless steel).
[0053] 1) By stamping a 304 stainless steel plate with a thickness of 1 mm, a punching net of an integral X-type lattice corresponding to the target X-type lattice is prepared, and the punching net has diamond-shaped holes;
[0054] 2) Using a stamping die corresponding to the target X-shaped lattice to stamp the above-mentioned punching net to prepare an integral X-shaped lattice;
[0055] 3) Cut the integral metal lattice by wire cutting, and prepare such as Figure 4 The split X-shaped lattice core shown;
[0056] 4) Clean the prepared dot matrix 1 and fins 2 with a metal cleaning agent to remove oil and rust, put them in an oven, and dry them in an environment of 45-55°C, and then put the fins 2 and dot matrix 1 according to figure 2 Assembly fixed;
[0057] 5) Clean the panel 3 with a metal cleaning agent to remove oil and rust, put it in an oven, dry it at 45-55°C, and mi...
Embodiment 2
[0062] Embodiment 2: as figure 1 Preparation of the sandwich panel shown (in aluminum).
[0063] 1) By stamping a 1060 series aluminum plate with a thickness of 1mm, a punching net corresponding to the target X-shaped lattice is prepared, the punching net has diamond-shaped holes, and there is no equal section at the intersection node of the punching net;
[0064] 2) Using a stamping die corresponding to the target X-shaped lattice to stamp the above-mentioned punching net to prepare an integral X-shaped lattice;
[0065] 3) Cut the integral metal lattice by wire cutting, and prepare such as Figure 4 The split X-shaped lattice core shown;
[0066] 4) Clean the prepared dot matrix 1 and fins 2 with a metal cleaning agent to remove oil and rust, put them in an oven, and dry them in an environment of 45-55°C, and then put the fins 2 and dots together Array 1 according to figure 2 Assembly fixed;
[0067] 5) Clean the panel 3 with a metal cleaning agent to remove oil and ru...