Embodiment 1
[0191] A mixture of the following compositions was uniformly stirred and mixed, and then filtered through a 1 μm filter to obtain an alkali-developing type cyan coloring composition 1 .
[0192] Pigment dispersion 1 shown in Table 2 12.0 parts
[0193] Pigment dispersion 9 shown in Table 2 48.0 parts
[0194] Photopolymerization initiator 2.0 parts
[0195] ("IRGACURE" 907 manufactured by Ciba Specialty Chemicals)
[0196] Trimethylolpropane triacrylate 5.0 parts
[0197] ("NK ESTER ATMPT" produced by Shin-Nakamura Chemical Co., Ltd.)
[0198] 0.5 parts of sensitizer
[0199] ("EAB-F" produced by Hodo Keya Chemical Co., Ltd.)
[0200] Acrylic resin solution 1 2.5 parts
[0201] Cyclohexanone 30.0 parts
Embodiment 2-20、 comparative example 1-3
[0203] Except using the pigment dispersion shown in Table 3, following the same method as Example 1, cyan or yellow coloring composition 2-20 was obtained.
[0204]
[0205] Coloring compositions 16-19 were obtained in the same manner as in Example 1 except that the pigment dispersions shown in Table 3 were used.
[0206] table 3
[0207]
coloring composition
Hue of the coloring composition
type
Quantity (parts)
type
Quantity (parts)
x
y
Y
Example 1
1
1
12
9
48
0.131
0.222
12.8
1500
2.7
Example 2
2
2
12
9
48
0.131
0.222
12.9
2000
2.9
Example 3
3
4
12
9
48
0.131
0.222
12....
Embodiment 11-24、 and comparative example 4-6
[0221]
[0222] A black matrix is processed to form a pattern on a glass substrate, and a coloring composition 17 is applied on the substrate with a spin coater to form a coating film of the coloring composition. Irradiate 300mJ / cm with an ultra-high pressure mercury lamp through a photomask on the film 2 of ultraviolet light. Next, the unexposed part was removed by spray development with an alkaline developer composed of 2% by weight of sodium carbonate aqueous solution, and then washed with ion-exchanged water, and the substrate was heated at 230°C for 20 minutes to form a film thickness of 2.5 μm. red filter section. In the same manner, green filter segments and blue filter segments having a film thickness of 2.5 μm were formed using coloring compositions 18 and 19 . In the same manner, coloring compositions 1-27 shown in Table 5 were used to form cyan, yellow, and magenta filter segments with a film thickness of 2.5 μm to produce color filters.
[0223]
[0224] U...
PUM
Property | Measurement | Unit |
---|---|---|
diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com