An anti-counterfeiting paper and coating technology, applied in the direction of specific visual effect coating, etc., can solve the problems of high requirements on construction machines and construction environment, poor holographic pattern reproducibility, poor printing adaptability, etc., to achieve strong light visual effect, good reproduction effect, Easy construction effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0021] A method for preparing a coating for packaging anti-counterfeiting paper, the method comprising the following process steps:
[0022] (1) First put all the solvents, namely 42 kg of ethyl acetate and 40 kg of methyl ethyl ketone into the reaction kettle, and heat to about 40°C for stirring;
[0023] (2) Keep stirring and put 10 kilograms of cellulose acetate butyrate resin and 6 kilograms of acrylic resin into the reaction kettle successively, and stir for about 1 hour;
[0024] (3) After mixing evenly, slowly put 2 kg of rosin resin into the reaction kettle; when no rosin resin is added, there will be no problem with commonly used offset printing, and gravure and flexographic printing may have poor ink adhesion It appears that the addition of rosin resin can improve the adhesion of the ink, so its printing application range is wide;
[0025] (4) When all the solids are dissolved and mixed evenly, shut down and mature for more than 12 hours;
[0026] (5) Measure the s...
Embodiment 2
[0030] A method for preparing a coating for packaging anti-counterfeiting paper, the method comprising the following process steps:
[0031] (1) First put all the solvents, namely 42 kg of ethyl acetate and 40 kg of methyl ethyl ketone into the reaction kettle, and heat to about 40°C for stirring;
[0032] (2) Keep stirring and drop 8 kilograms of cellulose acetate butyrate resin and 4 kilograms of nitrocellulose into the reaction kettle successively, and stir for about 1 hour;
[0033] (3) Slowly drop 3 kilograms of acrylic resin into the reaction kettle after mixing evenly;
[0034] (4) When all the solids are dissolved and mixed evenly, shut down and mature for more than 12 hours;
[0035] (5) Measure the solid content and adjust to the theoretical value;
[0036] (6) Stir slowly for about 1 hour, cool down, weigh and pack.
Embodiment 3
[0038] A method for preparing a coating for packaging anti-counterfeiting paper, the method comprising the following process steps:
[0039] (1) First put all the solvents, namely 42 kg of ethyl acetate and 40 kg of methyl ethyl ketone into the reaction kettle, and heat to about 40°C for stirring;
[0040] (2) Keep stirring and put 12 kilograms of cellulose acetate butyrate resin, 2 kilograms of nitrocellulose, and 3 kilograms of acrylic resin into the reaction kettle in turn, and stir for about 1 hour;
[0041] (3) Slowly drop 1 kilogram of rosin resin into the reaction kettle after mixing evenly;
[0042] (4) When all the solids are dissolved and mixed evenly, shut down and mature for more than 12 hours;
[0043] (5) Measure the solid content and adjust to the theoretical value;
[0044] (6) Stir slowly for about 1 hour, cool down, weigh and pack.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com