[0022] Embodiment 1 prepares catalyst
[0023] (1) 6.5mL of chloroplatinic acid solution and 11.9mL of ferric nitrate solution are mixed;
[0024] (2) At 80°C, by adding K 2 CO 3 solution, magnetically stirred for 2 hours, the catalytically active components were simultaneously precipitated, and left standing overnight;
[0025] (3) Suction filter the reaction solution obtained in (2), wash the filter residue, and dry at 80°C.
[0026] (4) Calcining the powder obtained in (3) in an air atmosphere at 400°C for 2h, that is, to obtain 5% loading of Pt / Fe 2 o 3 .
Embodiment 2
[0027] Embodiment 2 prepares catalyst
[0028] (1) 13.0mL chloroplatinic acid solution and 11.3mL ferric nitrate solution are mixed;
[0029] (2) At 80°C, by adding K 2 CO 3 solution, magnetically stirred for 2 hours, the catalytically active components were simultaneously precipitated, and left standing overnight;
[0030] (3) Suction filter the reaction solution obtained in (2), wash the filter residue, and dry at 80°C.
[0031] (4) Calcining the powder obtained in (3) in an air atmosphere at 400°C for 2 hours, that is, to obtain 10% loading of Pt / Fe 2 o 3 .
Embodiment 3
[0032] Embodiment 3 prepares catalyst
[0033] (1) 19.5mL chloroplatinic acid solution and 10.6mL ferric nitrate solution are mixed;
[0034] (2) At 80°C, by adding K 2 CO 3 solution, magnetically stirred for 2 hours, the catalytically active components were simultaneously precipitated, and left standing overnight;
[0035] (3) Suction filter the reaction solution obtained in (2), wash the filter residue, and dry at 80°C.
[0036] (4) Calcining the powder obtained in (3) in an air atmosphere at 400 ° C for 2 hours, that is, to obtain a Pt / Fe with a loading capacity of 15% 2 o 3 .
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com