Cationic fluorinated polymer compositions and methods of treating hydrocarbon-bearing formations using same

A technology of fluorinated polymer and composition, which can be used in drilling compositions, chemical instruments and methods, earth-moving drilling, etc., and can solve problems such as unsatisfactory downhole conditions

Inactive Publication Date: 2016-03-23
3M INNOVATIVE PROPERTIES CO
View PDF5 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0005] Solvent injection (such as methanol injection) has been used to alleviate water plugging and condensate accumulation problems in gas wells, but this method can only provide temporary benefits and may not be ideal for some downhole conditions

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Cationic fluorinated polymer compositions and methods of treating hydrocarbon-bearing formations using same
  • Cationic fluorinated polymer compositions and methods of treating hydrocarbon-bearing formations using same
  • Cationic fluorinated polymer compositions and methods of treating hydrocarbon-bearing formations using same

Examples

Experimental program
Comparison scheme
Effect test

example

[0195] In the following examples, MeFBSEA was prepared according to the method of Parts A and B of Example 2 of U.S. Patent No. 6,664,354 (Savu), except that 4270 kilograms (kg) of N-methylperfluorobutanesulfonamide ethanol, 1.6 kg phenothiazine, 2.7 kg methoxyhydroquinone, 1590 kg heptane, 1030 kg acrylic acid, 89 kg methanesulfonic acid (in place of trifluoromethanesulfonic acid) and 7590 kg water (in part B).

[0196] In the following examples, 3,3,4,4,5,5,6,6,7,7,8,8,8-tridecafluorooctyl acrylate (FOA) was prepared according to the following method. Add 100 g (0.275 mol) of 1H,1H,2H,2H-perfluorooct-1-ol (C 6 f 13 C 2 h 4 OH) (available from Clariant Chemical Co. (Mount Holly, NC) under the trade designation "FLUOWETEA 600"), 19.8 grams (0.275 moles) of acrylic acid (available from Sigma-Aldrich (St. Louis, MO)), 250 grams of heptane, and 1 gram of methane sulfonic acid, and the mixture was heated to reflux for 15 hours. Water (approximately 4.9 to 5 grams) was collect...

example 6 and 7

[0204] The preparation of Examples 6 and 7 was carried out according to the method of Examples 1 to 5, except that 30 grams of solvent mixture was used, the amounts of reagents used and the molar and weight ratios are given in Table 3 below.

[0205] table 3

[0206]

[0207] The gram loss during polymerization and the percent solids of the resulting polymer are given in Table 3 above.

[0208] Examples 8 to 11

[0209] Into each of five 0.1 liter (4 oz) pressure bottles was placed DMAEAMCl (80% by weight in water, available from Ciba Specialty Chemicals under the trade designation "CIBAAGEFLEXFA1Q80MC") and MeFBSEA or FOA in the amounts shown in Table 4 below. For Examples 8 and 9, a mixture of 90 grams of methanol, 90 grams of methyl ethyl ketone, 3 grams of 3-mercapto-1,2-propanediol and 0.60 grams of 2,2'-azobis(2-methylbutyronitrile) was prepared batch. For Examples 10 and 11, a mixture of 45 grams of methanol, 45 grams of methyl ethyl ketone, 1.5 grams of 3-mer...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
diameteraaaaaaaaaa
porosityaaaaaaaaaa
Login to View More

Abstract

The present invention discloses a fluorinated polymer having a first divalent unit independently represented by formula (I): or formula (II) and a second divalent unit containing a quaternary ammonium group. Compositions comprising fluorinated polymers and solvents, methods of treating hydrocarbon-bearing formations using these compositions, and fluorinated polymer-treated articles are disclosed. Also disclosed are methods of making compositions containing fluorinated polymers.

Description

[0001] Cross References to Related Applications [0002] This application claims priority to US Provisional Application Serial No. 61 / 081826, filed July 18, 2008, the contents of which are incorporated herein by reference. Background technique [0003] In the oil and gas industry, certain surfactants, including certain fluorinated surfactants, are known fluid additives for various downhole operations such as fracturing, water injection and drilling. Typically, these surfactants act to lower the surface tension of the fluid or to stabilize the foaming fluid. [0004] Some hydrocarbons and fluorine-containing compounds have been used to modify the wettability of reservoir rocks, which can be used, for example, to avoid or remedy water plugging (eg, in oil or gas wells) near the wellbore (ie, in the region near the wellbore) or liquid Hydrocarbon accumulation (eg, in gas wells). Water plugging and liquid hydrocarbon accumulation may be caused by natural phenomena (eg, water-be...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): C08F220/34C08F220/38E21B43/22
CPCC08F220/34E21B43/25C09K8/60C09K8/88C09K8/604C08F220/387C08F220/24
Inventor 小吉米·R·巴兰乔治·G·I·莫尔
Owner 3M INNOVATIVE PROPERTIES CO