Preparation method of building material containing waste fiber
A technology for building materials and waste fibers, which is used in the field of construction and materials to improve earthquake resistance, enhance flexibility, and solve tight supply and demand.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment approach 1
[0015] I. adopt, slag, fly ash, river sand, lime, cement material are as initial material, and initial formula is: cement 530kg, middle sand 348kg, gravel 845kg, water: 220kg;
[0016] II. The ingredient scheme is as follows:
[0017] Cement: 424kg, medium sand: 348kg, gravel: 845kg, slag: 53kg, fly ash 53kg, water-cement ratio: 1:0.3, waste fiber: fiber volume accounts for 2% of the total material volume;
[0018] III. Optimization and determination of combined integrated block structure
[0019] There are no special requirements and restrictions on the size and shape of the test block, which can be determined according to actual needs. Generally, it is 36×24×18.5cm, and the molding pressure is 20KN. After molding, it should be cured under natural conditions and heat preservation conditions. After 28 days, Carry out a pressure test with a strength of 25MP.
Embodiment approach 2
[0021] I. adopt, slag, fly ash, river sand, lime, cement material are as initial material, and initial formula is: cement 530kg, middle sand 348kg, gravel 845kg, water: 220kg;
[0022] II. The ingredient scheme is as follows:
[0023] Cement: 424kg, medium sand: 348kg, gravel: 845kg, slag: 53kg, fly ash 53kg, water-cement ratio: 1:0.3, waste fiber: fiber volume accounts for 0.5% of the total material volume;
[0024] III. Optimization and determination of combined integrated block structure
[0025] There are no special requirements and restrictions on the size and shape of the test block. According to actual needs, it is determined to be 18×12×9.5cm, and the molding pressure is 15KN. After molding, it is maintained under natural conditions and heat preservation conditions. Strength is 112.08MP.
Embodiment approach 3
[0027] I. adopt, slag, fly ash, river sand, lime, cement material are as initial material, and initial formula is: cement 530kg, middle sand 348kg, gravel 845kg, water: 220kg;
[0028] II. The ingredient scheme is as follows:
[0029] Cement: 318kg, medium sand: 348kg, gravel: 845kg, slag: 106kg, fly ash 106kg, water-cement ratio: 1:0.3, waste fiber: fiber volume accounts for 2% of the total material volume;
[0030] III. Optimization and determination of combined integrated block structure
[0031] The size of the test block is determined to be 40×40×40cm according to actual needs, and the molding pressure is 20KN. After molding, it is maintained under natural conditions and heat preservation conditions. After 28 days, a pressure test is carried out, and the strength is 14.75MP.
[0032] Embodiment 3
[0033] I. adopt, slag, fly ash, river sand, lime, cement material are as initial material, and initial formula is: cement 530kg, middle sand 348kg, gravel 845kg, water: 220kg...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com