Dihydrate desulfurized gypsum water-resistant putty for interior and exterior walls, and production method thereof
A desulfurized gypsum and production method technology, applied in the field of desulfurized gypsum and solid waste, can solve the problems of secondary energy consumption, poor water resistance, high cost, etc., and achieve the effects of reasonable crystal shape, enhanced water resistance, and improved water resistance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0039] In this example, the ratio of raw materials for dihydrate desulfurized gypsum water-resistant interior wall putty is as follows:
[0040] 1. Original dihydrate desulfurization gypsum: 65%
[0041] Fly ash: 3%
[0043] Cement: 7.0%
[0045] Slag fine powder: 23.0%
[0046] The above constitutes a composite gelling material.
[0047] 2. Dihydrate desulfurization gypsum water-resistant interior wall putty (JC / T3049-1998)
[0048] Composite cementitious material: 62%
[0049] Sulphoaluminate cement: 5%
[0050] Ground calcium carbonate: 30%
[0051] Hydroxypropyl methylcellulose ether: 0.2%
[0052] Tapioca starch: 3.0%
[0053] Pwc500: 0.2%
[0054] After testing: grinding property: 40%, bonding strength: 0.6mpa, flexural strength: 3.1mpa, compressive strength: 8.9mpa, softening coefficient: 0.6.
[0055] The dihydrate desulfurization gypsum water-resistant interior wall putty provided in the present inve...
Embodiment 2
[0061] In this case, the dihydrate desulfurization gypsum water-resistant exterior wall putty, the raw material formula is as follows:
[0062] 1. Original dihydrate desulfurization gypsum: 66.5%
[0063] Slag fine powder: 24%
[0065] Cement: 8.0%
[0067] The above constitutes a composite gelling material.
[0068] 2. Dihydrate desulfurization and water-resistant exterior wall putty (JC / T157-2004)
[0069] Composite cementitious material: 65%
[0070] Sulphoaluminate cement: 3%
[0071] Ground calcium carbonate: 30.5%
[0072] Hydroxypropyl methylcellulose ether: 0.2%
[0073] Rubber powder 5044N: 1.5%
[0074] Pwc500: 0.3%
[0075] The above composition dihydrate desulfurization gypsum water-resistant exterior wall putty.
[0076] After testing: bonding strength: 0.65mpa, flexural strength: 3.8mpa, compressive strength: 9.8mpa, softening coefficient: 0.75.
[0077] The dihydrate desulfurized gypsum wate...
PUM
Property | Measurement | Unit |
---|---|---|
compressive strength | aaaaa | aaaaa |
flexural strength | aaaaa | aaaaa |
compressive strength | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com