Embodiment 1
[0042] The preparation method of environmentally friendly non-floating aluminum-silver paste pigment, the steps are as follows:
[0043] 1. Preparation of solvent: take 3 kg of butyl acetate; 2 kg of methyl ethyl ketone; 2 kg of methyl isobutyl ketone; 3 kg of ethanol and mix well.
[0044] 2. Ball milling: Take 10 kilograms of spherical aluminum powder and mix it in 10 kilograms of solvent. Stir slowly for 20 minutes until uniformly mixed. Put into a ball mill for grinding, the ball mill rotates at 37 revolutions per minute, the internal temperature is 50-55°, and the casing temperature is 40-45° to make flake particles; the pigment flake particle suspension is transported to the storage material through the pipeline with vacuum pressure Tank precipitation.
[0045] 3. Sieving: Put the ball milled product into a sieving machine with a screen mesh of 100 meshes to obtain flake pigments; the sieved pigment suspension is transported to the storage tank for precipitation by vacuum air ...
Embodiment 2
[0051] The preparation method of environmentally friendly non-floating aluminum-silver paste pigment, the steps are as follows:
[0052] 1. Preparation of solvent: take 3 kg of butyl acetate; 2 kg of methyl ethyl ketone; 2 kg of methyl isobutyl ketone; 3 kg of ethanol and mix well.
[0053] 2. Ball milling: Take 8 kilograms of spherical aluminum powder and mix it in 10 kilograms of solvent. Stir slowly for 15 minutes until uniformly mixed. Put into a ball mill for grinding, the ball mill rotates at 37 revolutions per minute, the internal temperature is 50-55°, and the casing temperature is 40-45° to make flake particles; the pigment flake particle suspension is transported to the storage material through the pipeline with vacuum pressure Tank precipitation.
[0054] 3. Sieving: Put the ball milled product into a sieving machine with a screen mesh of 400 meshes to obtain flake pigments; the sieved pigment suspension is transported to the storage tank for precipitation by vacuum air p...
Embodiment 3
[0060] The preparation method of environmentally friendly non-floating aluminum-silver paste pigment, the steps are as follows:
[0061] 1. Preparation of solvent: take 3 kg of butyl acetate; 2 kg of methyl ethyl ketone; 2 kg of methyl isobutyl ketone; 3 kg of ethanol and mix well.
[0062] 2. Ball milling: Take 6 kilograms of spherical aluminum powder and mix it in 10 kilograms of solvent. Stir slowly for 10 minutes until uniformly mixed. Put into a ball mill for grinding, the ball mill rotates at 37 revolutions per minute, the internal temperature is 50-55°, and the casing temperature is 40-45° to make flake particles; the pigment flake particle suspension is transported to the storage material through the pipeline with vacuum pressure Tank precipitation.
[0063] 3. Sieving: Put the ball milled product into a sieving machine with a screen mesh of 500 meshes to obtain particle size flake pigments; the sieved pigment suspension is transported to the storage tank for precipitation b...