Heavy water reactor fuel canning graphite emulsion paint and preparation method thereof
A fuel cladding and graphite emulsion technology, applied in epoxy resin coatings, coatings, etc., can solve problems such as pores in end plug materials and excessive hydrogen content in components, and achieve good construction performance, satisfactory volatilization speed, and reasonable particle size distribution. Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0023] Raw materials (mass percentage): 25% of graphite powder, 20% of thermoplastic acrylic resin, 1.5% of epoxy resin, 1.5% of fumed silica, and 52% of mixed solvent. In the solvent, isopropanol 90%, terpineol 5%, n-butanol 5%.
[0024] The preparation method is as follows:
[0025] (1) Preparation of mixed solvent: Weigh 46.8g of isopropanol, 2.6g of terpineol, and 2.6g of n-butanol, stir in a stirring tank, dissolve and mix evenly;
[0026] (2) Add 20g of thermoplastic acrylic resin and 1.5g of epoxy resin, stir and fully dissolve;
[0027] (3) Add 1.5 g of fumed silica, stir and mix evenly;
[0028] (4) 25g of graphite powder is dropped into the stirring tank, stirred until uniformly mixed;
[0029] (5) Transfer the uniform slurry in the stirring tank to a rolling mill, and roll it for 1 to 4 hours to form a uniform graphite emulsion, pass through a 100-mesh sieve, and pack.
Embodiment 2
[0031] Raw materials (mass percentage): graphite powder 20%, styrene-acrylic resin 14%, dibutyl phthalate 0.5%, polyamide wax 6900-20X 0.5%, mixed solvent 65%. In the solvent, isopropanol 85%, n-butanol 5%, hexanediol 5%, propylene glycol methyl ether 5%.
[0032] The preparation method is as follows:
[0033] (1) Preparation of mixed solvent: Weigh 55.25g of isopropanol, 3.25g of n-butanol and 3.25g of hexanediol, stir in a stirring tank, dissolve and mix evenly;
[0034] (2) Add 14g of styrene-acrylic resin and 0.5g of dibutyl phthalate, stir and fully dissolve;
[0035] (3) Add polyamide wax 6900-20X 0.5g, stir and mix evenly;
[0036] (4) 20g of graphite powder is dropped into the stirring tank, stirred until evenly mixed;
[0037] (5) Transfer the uniform slurry in the stirring tank to a rolling mill, and roll it for 1 to 4 hours to form a uniform graphite emulsion, pass through a 100-mesh sieve, and pack.
Embodiment 3
[0039] Raw materials (mass percentage): graphite powder 16%, ethyl cellulose 4%, dibutyl phthalate 0.25%, hydroxy acrylate 0.25%, gas phase SiO 2 0.5%, mixed solvent 79%. In the solvent, isopropanol 95%, hexanediol 1.25%, n-butanol 1.25%, propylene glycol methyl ether 1.25%, ethylene glycol 1.25%.
[0040] The preparation method is as follows:
[0041] (1) Preparation of mixed solvent: Weigh 75.05g of isopropanol, 0.9875g of hexanediol, 0.9875g of n-butanol, 0.9875g of propylene glycol methyl ether, and 0.9875g of ethylene glycol, and place them in a stirring tank to stir, dissolve, well mixed;
[0042] (2) Add 4 g of ethyl cellulose, 0.25 g of dibutyl phthalate, and 0.25 g of hydroxyacrylate, stir and fully dissolve;
[0043] (3) Add gas phase SiO 2 0.5g, stir and mix evenly;
[0044] (4) Graphite powder 16g is dropped in the mixing tank, stirs to mix evenly;
[0045] (5) Transfer the uniform slurry in the stirring tank to a rolling mill, and roll it for 1 to 4 hours t...
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com