Circularly-tanning technology for chrome tanning liquor of sheep garment leather
A technology for liquid circulation and wool leather, which is applied in the field of chrome tanning liquid circulation tanning process, can solve the problems of fluctuation in the quality of raw leather, production of hexavalent chromium, flocculation, etc., and achieve the effect of bright color, enhanced fatliquoring effect, and pure white coat color.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0039] A kind of chrome liquid circulation tanning process of sheep clothing hair leather, comprises the following steps:
[0040] Step 1, rewetting: before shearing, the sheep skin is rehydrated with a salt solution with a concentration of 80g / L at 35°C, the mass ratio of water to fur is 30, and the soaking time is 4 hours;
[0041] Step 2, drying, using a drying machine to remove excess water in the skin;
[0042] Step 3, shearing, use a shearing machine to shear the wool to make the plush fluffy, basically remove dirt and dust, and recycle the sheared wool;
[0043] Step 4, main immersion: Soak the sheepskin after shearing. The mass ratio of water to fur in the soaking solution is 20. The soaking solution is measured by water volume, including 1.5g / L of preservative, 25g / L of table salt, and 1.0g / L of penetrant. L, temperature 20°C, soak overnight for 14 hours;
[0044] Step 5, remove the flesh, after soaking in water, remove the remaining meat film on the surface of the ...
Embodiment 2
[0064] A kind of chrome liquid circulation tanning process of sheep clothing hair leather, comprises the following steps:
[0065] Step 1, rewetting: before shearing, the sheep skin is rehydrated with a salt solution with a concentration of 40g / L at 30°C, the mass ratio of water to fur is 20, and the soaking time is 4 hours;
[0066] Step 2, drying, using a drying machine to remove excess water in the skin;
[0067] Step 3, shearing, use a shearing machine to shear the wool to make the plush fluffy, basically remove dirt and dust, and recycle the sheared wool;
[0068] Step 4, main immersion: Soak the sheared sheepskin. The mass ratio of water to fur in the soaking solution is 20. The soaking solution is measured by water volume, including 1.5g / L of preservative, 15g / L of salt, and 1.0g / L of penetrant. L, temperature 20°C, soak overnight for 14 hours;
[0069] Step five, remove the meat;
[0070] Step 6, degreasing: the mass ratio of water to fur in the degreasing solution ...
Embodiment 3
[0091] A kind of chrome liquid circulation tanning process of sheep clothing hair leather, comprises the following steps:
[0092] Step 1, rewetting: before shearing, the sheepskin is rehydrated with a salt solution with a concentration of 30g / L at 30°C, the mass ratio of water to fur is 20, and the soaking time is 2h;
[0093] Step 2, spin dry;
[0094] Step three, shearing;
[0095] Step 4, main immersion: Soak the sheepskin after shearing. The mass ratio of water to fur in the soaking solution is 20. The soaking solution is measured by water volume, including 0.5g / L of preservative, 10g / L of table salt, and 0.5g / L of penetrant. L, temperature 20°C, soak overnight for 12 hours;
[0096] Step five, remove the meat;
[0097] Step 6, degreasing: the mass ratio of water to fur in the degreasing solution is 20, and the degreasing solution is measured by water volume, including 0.5 g / L of soda ash, 2 g / L of degreasing agent, and 0.5 g / L of penetrating agent, at a temperature of...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology