A chrome-free tanning agent and chrome-free tanning technology, applied in the treatment of small raw hide/big raw hide/leather/fur, chemical treatment and application of small raw hide/big raw hide/leather skin/fur, and can solve the problem of reducing curl, chrome Tanning cannot maintain naturalness, formaldehyde tanning has high content of free formaldehyde, etc., to achieve the effect of reducing treatment costs, leather body feels plump, and hair color is pure white
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0046] Step 1, soaking in water: Soak the beach sheepskin in a 35°C soaking solution 20 times its mass for 12 hours;
[0047] Each liter of soaking liquid contains 0.5g fungicide ECOGRIN30LR (Tiger Leather Chemical), 18g salt (NaCl), 0.5g degreasing agent ACTOL DB (ATC Leather Chemical) and 0.1g soaking enzyme Feliderm SE3Powder (Clariant Chemical);
[0048] Step 2, removing the flesh from the beach sheepskin soaked in the soaking liquid;
[0049] Step three, degreasing:
[0050] Place the de-fleshed fur in a 35°C degreasing solution 20 times its mass, and paddle for 30 minutes;
[0051] Each liter of the degreasing solution contains 0.5g of soda ash, 0.1g of compound enzyme LTK-100 (Shenzhen Lvweikang Biological Engineering Co., Ltd.), 0.5g of penetrant JFC (Zibo Haijie Chemical Industry) and 2g of degreasing agent PX (Sheng Hui Chemical Industry);
[0052] Step four, soften:
[0053]Add alkaline softening enzyme JB-Ⅱ (Xuzhou Tianli Enzyme Preparation Co., Ltd.) to the de...
Embodiment 2
[0084] Step 1, soaking in water: Soak the beach sheepskin in a 30°C soaking solution 25 times its mass for 24 hours;
[0085] Each liter of soaking liquid contains 1.0g of fungicide ECOGRIN30LR (Tiger Leather Chemical), 10g of salt (NaCl), 1.5g of degreasing agent ACTOL DB (ATC Leather Chemical) and 0.8g of soaking enzyme FelidermSE3Powder (Clariant Chemical);
[0086] Step 2, removing the flesh from the beach sheepskin soaked in the soaking liquid;
[0087] Step three, degreasing:
[0088] Place the de-fleshed fur in a 38°C degreasing solution that is 30 times its mass, and paddle for 80 minutes;
[0089] Each liter of degreasing solution contains 1.0g of soda ash, 1.5g of compound enzyme LTK-100 (Shenzhen Lvweikang Biological Engineering Co., Ltd.), 1.0g of penetrant JFC (Zibo Haijie Chemical Industry) and 3g of degreasing agent PX (Sheng Hui Chemical Industry);
[0090] Step four, soften:
[0091] Add alkaline softening enzyme JB-Ⅱ (Xuzhou Tianli Enzyme Preparation Co.,...
Embodiment 3
[0122] Step 1, soaking in water: Soak the beach sheepskin in a 32°C soaking solution that is 30 times its mass for 18 hours;
[0123] Each liter of soaking liquid contains 1.5g of fungicide ECOGRIN30LR (Tiger Leather Chemical), 25g of salt (NaCl), 2.5g of degreasing agent ACTOL DB (ATC Leather Chemical) and 1.5g of soaking enzyme FelidermSE3Powder (Clariant Chemical);
[0124] Step 2, removing the flesh from the beach sheepskin soaked in the soaking liquid;
[0125] Step three, degreasing:
[0126] Place the de-fleshed fur in a degreasing solution at 40°C that is 40 times its mass, and paddle for 120 minutes;
[0127] Each liter of degreasing solution contains 1.5g of soda ash, 0.8g of complex enzyme LTK-100 (Shenzhen Lvweikang Biological Engineering Co., Ltd.), 1.5g of penetrant JFC (Zibo Haijie Chemical Industry) and 5g of degreasing agent PX (Sheng Hui Chemical Industry);
[0128] Step four, soften:
[0129] Add alkaline softening enzyme JB-Ⅱ (Xuzhou Tianli Enzyme Prepa...
PUM
Property | Measurement | Unit |
---|---|---|
temperature | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com