Clear wood paint and preparation method thereof

A wood lacquer, clear technology, used in coatings, polyurea/polyurethane coatings, etc., can solve problems such as poor transparency and whitening of the paint film, and achieve the effect of strong adhesion, clear paint film, and strong paint film

Active Publication Date: 2013-06-05
NIPPON PAINT CHENGDU
View PDF3 Cites 7 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0003] The object of the present invention is to provide a kind of clear wood paint and its preparation method, to solve the problems of extrem

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Clear wood paint and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

Example Embodiment

[0039] Example 1

[0040] A clear wood lacquer, which is composed of component A and component B in a weight ratio of 1:0.5; The finished product or the trimer of TDI or their mixture, 18% of butyl acetate and 18% of ethyl acetate; the component B is composed of 65.9% by weight of alkyd resin or modified alkyd resin or Their mixture, 2.55% butyl acetate, 2.55% ethyl acetate, 2.55% xylene, 0.3% defoamer (BYK066, BYK), 0.35% leveling agent (BYK310, BYK) ), 10.8% matting agent (ED30, Grace), 4% antibacterial agent, 0.2% dispersant (EFKA-4010, Ciba Refinery (China) Co., Ltd.), 0.8% anti-settling agent (DISPARLON A -630-20X, Disparon) and 10% modified resin (25% 1 / 2S nitrocellulose solution, Weiye Chemical).

[0041] Its preparation method is as follows:

[0042] Preparation of Component A:

[0043] (1) Fill the tank with nitrogen for 5min, keep the pressure at 0.01~0.05Mpa, then put in 18% butyl acetate and 18% ethyl acetate by weight, and stir at low speed for 5min;

[0044]...

Example Embodiment

[0050] Example 2

[0051]A clear wood lacquer, which is composed of component A and component B in a weight ratio of 1:0.5; The finished product or the trimer of TDI or their mixture, 15% of butyl acetate and 15% of ethyl acetate; the component B is composed of 79% by weight of alkyd resin or modified alkyd resin or Their mixture, 0.5% butyl acetate, 0.5% ethyl acetate, 0.5% xylene, 0.36% defoamer (BYK066, BYK), 0.4% leveling agent (BYK310, BYK) ), 4.44% matting agent (ED30, Grace), 5% antibacterial agent, 0.3% dispersant (EFKA-4010, Ciba Refinery (China) Co., Ltd.), 1% anti-settling agent (DISPARLON A -630-20X, Disparon) and 8% modified resin (25% 1 / 2S nitrocellulose solution, Weiye Chemical).

[0052] Its preparation method is as follows:

[0053] Preparation of Component A:

[0054] (1) Fill the tank with nitrogen for 5min, keep the pressure at 0.01~0.05Mpa, then put in 15% butyl acetate and 15% ethyl acetate by weight, and stir at low speed for 5min;

[0055] (2) Unde...

Example Embodiment

[0061] Example 3

[0062] A clear wood lacquer, which is composed of component A and component B in a weight ratio of 1:0.25; the component A is composed of 30% by weight of toluene diisocyanate TDI and trimethylolpropane The finished product or the trimer of TDI or their mixture, 35% of butyl acetate and 35% of ethyl acetate; the component B is composed of 58% by weight of alkyd resin or modified alkyd resin or Their mixture, 3% butyl acetate, 3% ethyl acetate, 3% xylene, 0.16% defoamer (BYK066, BYK), 0.2% leveling agent (BYK310, BYK) ), 12.5% ​​matting agent (ED30, Grace), 5% antibacterial agent, 0.1% dispersant (EFKA-4010, Ciba Refinery (China) Co., Ltd.), 0.04% anti-settling agent (DISPARLON A -630-20X, Disparon) and 15% modified resin (25% 1 / 2S nitrocellulose solution, Weiye Chemical).

[0063] Its preparation method is as follows:

[0064] Preparation of Component A:

[0065] (1) Fill the tank with nitrogen for 5min, keep the pressure at 0.01-0.05Mpa, then put in 35%...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The invention discloses a clear wood paint and a preparation method thereof, belonging to the technical field of application of paints. The invention solves the problem of poor transparency of the wood paint in the construction process, and the problem of white paint film after recoating. The clear wood paint is composed of a component A and a component B, wherein the component A is composed of an addition product of toluene diisocyanate (TDI) and trimethylolpropane or TDI tripolymer or mixture thereof, butyl acetate and ethyl acetate; the component B is composed of alkyd resin or modified alkyd resin or mixture thereof, butyl acetate, ethyl acetate, dimethylbenzene, defoaming agent, leveling agent, flatting agent, antimicrobial agent, dispersing agent, anti-settling agent and modified resin; and the weight ratio of the component A to the component B is 1:0.5 or 1:0.25. The invention also provides a preparation method of the wood paint. The wood paint disclosed by the invention has the advantage of clear and layered paint film, and can better display the beautiful texture of the wood.

Description

technical field [0001] The invention belongs to the technical field of coating application, and in particular relates to a clear wood varnish and a preparation method thereof. Background technique [0002] In the product composition of wood coatings in my country, solvent-based products still occupy an important position. In solvent-based wood coatings, polyurethane coatings account for more than 90%, of which two-component polyurethane is the main one, but the transparency of the product during construction is extremely poor, and the phenomenon of whitening of the paint film after recoating is more prominent, which can no longer satisfy people. demand. Contents of the invention [0003] The object of the present invention is to provide a clear wood paint and its preparation method, which can solve the problems of extremely poor transparency of the wood paint during construction and whitening of the paint film after recoating in the prior art. [0004] In order to achiev...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
IPC IPC(8): C09D175/06C09D175/14C09D7/12
Inventor 谢飞
Owner NIPPON PAINT CHENGDU
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products