A kind of preparation method of fiber insulation board
A technology of thermal insulation board and fiber, applied in thermal insulation, textiles and papermaking, non-woven fabrics, etc., can solve the problems of easy combustion, poor safety, aging resistance, etc., to reduce the radiation of radioactive elements, reduce the interference of environmental noise, The effect of reducing the use of tiles
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0024] A method for preparing a fiber insulation board includes the following steps:
[0025] (A) Add the first polyester staple fiber and the second polyester staple fiber to the raw material feeding device, and the fibers are evenly mixed through the feeding device. The first polyester staple fiber accounts for 50% of the total fiber mass;
[0026] (B) Pre-open the mixed fibers to make the agglomerated fibers loose; after the pre-opening is completed, perform fine-opening to make the fibers uniformly mixed together; the opened fibers are compressed The device is fed into the carding equipment, and the fibers form a continuous fiber web after the carding equipment;
[0027] (C) Spray the flame retardant SAF8078 produced by Shanghai Huter Group Co., Ltd., which accounts for 2% of the total fiber mass, on the surface of the fiber web evenly;
[0028] (D) The fiber web processed in step (c) is subjected to needle punching, rolling, and heat setting to obtain an insulation board;
[0029]...
Embodiment 2
[0032] A method for preparing a fiber insulation board includes the following steps:
[0033] (A) Add the first polyester staple fiber and polyamide fiber to the raw material feeding device, and the fibers are evenly mixed through the feeding device, and the first polyester staple fiber accounts for 70% of the total fiber mass;
[0034] (B) Pre-open the mixed fibers to make the agglomerated fibers loose; after the pre-opening is completed, perform fine-opening to make the fibers uniformly mixed together; the opened fibers are compressed The device is fed into the carding equipment, and the fibers form a continuous fiber web after the carding equipment;
[0035] (C) Evenly spray the flame retardant CN-220 produced by Changshu Yongdeli Spunlace Nonwoven Co., Ltd. which accounts for 10% of the total fiber mass on the surface of the fiber web;
[0036] (D) The fiber web processed in step (c) is subjected to needle punching, rolling, and heat setting to obtain an insulation board;
[0037] ...
Embodiment 3
[0040] A method for preparing a fiber insulation board includes the following steps:
[0041] (A) Add the first polyester short fiber and carbon fiber to the raw material feeding device, and the fiber is evenly mixed through the feeding device. The first polyester short fiber accounts for 60% of the total fiber mass;
[0042] (B) Pre-open the mixed fibers to make the agglomerated fibers loose; after the pre-opening is completed, perform fine-opening to make the fibers uniformly mixed together; the opened fibers are compressed The device is fed into the carding equipment, and the fibers form a continuous fiber web after the carding equipment;
[0043] (C) Evenly spray the flame retardant Doher-6503 produced by Dongguan Saiensi Industrial Co., Ltd., which accounts for 6% of the total fiber mass, onto the surface of the fiber mesh;
[0044] (D) The fiber web processed in step (c) is subjected to needle punching, rolling, and heat setting to obtain an insulation board;
[0045] The needlin...
PUM
| Property | Measurement | Unit |
|---|---|---|
| melting point | aaaaa | aaaaa |
| melting point | aaaaa | aaaaa |