A technology of glass-ceramic and plate, which is applied in the field of black glass-ceramic plate and its production, can solve the problems of high energy consumption, restricting the rapid development and large-scale production of glass-ceramic, and achieve stable chemical composition and low production cost Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0023] According to another embodiment of the present invention, the production method of black glass-ceramic comprises the following steps:
[0024] 1. Select raw materials according to the following parts by weight, and send them to the mixer for mixing. The mixing time is 4 minutes, and 10Kg of water is added.
[0025] raw material name
Magnesite
granite
Calcium Dihydrogen Phosphate
heavy calcium
manganese ore
Weight (Kg)
94
348.6
17.7
27.5
36.8
[0026] Table 1: Chemical composition of raw materials (weight percent)
[0027] chemical composition
granite
heavy calcium
Iron oxide red
Magnesite
Calcium Dihydrogen Phosphate
Na 2 o
3.706
0
0
0.043
0
MgO
0.2687
0
0
42.7094
0
Al 2 o 3
11.7
0
0
0.2678
0
SiO 2
77.306
0
0
1.3426
0
P 2 o 5
0.0193
0
0
...
Embodiment 2
[0037] According to another embodiment of the present invention, the production method of black glass-ceramic comprises the following steps:
[0038] 1. Select raw materials according to the following parts by weight, and send them to the mixer for mixing. The mixing time is 4 minutes, and 10Kg of water is added.
[0039] raw material name
Magnesite
granite
Calcium Dihydrogen Phosphate
heavy calcium
manganese ore
Weight (Kg)
88.7
348.7
19.5
30.4
35.8
[0040] 2. Send the above-mentioned mixture into the melting pool of the all-electric melting furnace, control the melting temperature to 1400°C, and clarify and homogenize the melted glass. The temperature of clarification and homogenization is 1400°C. The time is 8h.
[0041] 3. The clarified and homogenized glass enters the forehearth through the flow hole and the ascending channel, and the temperature drops to 1300°C. After cooling down through the forehearth, i...
PUM
Property | Measurement | Unit |
---|---|---|
compressive strength | aaaaa | aaaaa |
flexural strength | aaaaa | aaaaa |
density | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com