A kind of uv ink layer with raindrop effect and manufacturing method thereof
An ink layer, ink technology, applied in ink, chemical instruments and methods, household appliances, etc., can solve problems such as physical and mental health hazards
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0030] Preparation of the first layer of ink:
[0031] 1. Ingredients: Take 10 parts of functional acrylate active monomer.
[0032] 1) In a certain volume of agitable open tank, 10 parts of functional acrylate active monomer and 3 parts of initiator are pre-dispersed for 20 minutes at medium speed (200rpm) with a disk-type stirring paddle, and the initiator is required to be fully dissolved.
[0033] 2) Add 20 parts of polyurethane acrylate, 2 parts of hydroxyl polyester acrylic resin, 5 parts of epoxy acrylic resin, 0.3 parts of leveling agent and 5 parts of wax powder.
[0034] 2. Dispersion: The mixture obtained in step 2 was dispersed for 40 minutes at high speed (3000 rpm) with a disc-type stirring paddle to obtain the first base ink.
[0035] 3. Grinding: Grind the dispersed first ingredient mixture with a hydraulic three-roller machine for 5 minutes, and the test fineness is less than 10 microns, and the first layer of ink is obtained.
[0036] Preparation of the sec...
Embodiment 2
[0044] Preparation of the first layer of ink:
[0045] 1. Ingredients: Take 18 parts of functional acrylate active monomer.
[0046] 1) In a certain volume of open tank that can be stirred, 18 parts of functional acrylate reactive monomer and 4 parts of initiator are pre-dispersed for 20 minutes at medium speed (200rpm) with a disk-type stirring paddle, and the initiator is required to be fully dissolved.
[0047] 2) Add 35 parts of polyurethane acrylate, 6 parts of hydroxyl polyester acrylic resin, 12 parts of epoxy acrylic resin, 0.6 parts of leveling agent and 7 parts of wax powder.
[0048] 2. Dispersion: The mixture obtained in step 2 was dispersed for 40 minutes at high speed (3000 rpm) with a disc-type stirring paddle to obtain the first base ink.
[0049] 3. Grinding: Use a hydraulic three-roll machine to grind the dispersed first ingredient mixture for 10 minutes, and the test fineness is less than 10 microns, and the first layer of ink is obtained.
[0050] Preparati...
Embodiment 3
[0058] Preparation of the first layer of ink:
[0059] 1. Ingredients: Take 25 parts of functional acrylate active monomer.
[0060] 1) In a certain volume of open tank that can be stirred, 25 parts of functional acrylate reactive monomer and 6 parts of initiator are pre-dispersed for 40 minutes at medium speed (200rpm) with a disk-type stirring paddle, and the initiator is required to be fully dissolved.
[0061] 2) Add 50 parts of polyurethane acrylate, 10 parts of hydroxyl polyester acrylic resin, 20 parts of epoxy acrylic resin, 1 part of leveling agent and 10 parts of wax powder.
[0062] 2. Dispersion: The mixture obtained in step 2 was dispersed for 40 minutes at high speed (3500 rpm) with a disc-type stirring paddle to obtain the first base ink.
[0063] 3. Grinding: Use a hydraulic three-roll machine to grind the dispersed first ingredient mixture for 15 minutes, and the test fineness is less than 10 microns, and the first layer of ink is obtained.
[0064] Preparat...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology