Environmentally-friendly organic photochromic aqueous polymer paint and preparation method thereof
A water-based polymer and photochromic technology, applied in the direction of multi-color effect coatings, coatings, etc., can solve the problem of single color
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
preparation example Construction
[0035] An environment-friendly organic photochromic water-based polymer coating and a preparation method thereof, comprising the following steps:
[0036] Step 1: Emulsion Preparation
[0037] Take 300-500Kg of distilled water, 8-10Kg of emulsifier OP-10, and 8-10Kg of sodium dodecylbenzenesulfonate into the reaction kettle, and stir thoroughly to dissolve the emulsifier in the water to form an emulsion.
[0038] The second step: Initiator preparation
[0039] Take 10-20Kg of ammonium persulfate, 3-5Kg of dibenzoyl peroxide (BPO), and 5-10Kg of distilled water into the mixing tank, and stir thoroughly.
[0040] Step 3: Synthesize Acrylic Emulsion
[0041] Take 100-150Kg of acrylic acid and 100-150Kg of n-butyl acrylate and slowly add them to the reaction kettle of the first step in three times, stir well, control the temperature of the solution to keep 65-70°C, and keep it constant, then add the 10 prepared in the second step - 15Kg initiator mixed solution, fully stirred f...
Embodiment 1
[0045] An environment-friendly organic photochromic water-based polymer coating and a preparation method thereof, comprising the following steps:
[0046] Step 1: Emulsion Preparation
[0047] Take 300Kg of distilled water, 80Kg of emulsifier OP-10, and 8Kg of sodium dodecylbenzenesulfonate into the reaction kettle, and stir thoroughly to dissolve the emulsifier in the water to form an emulsion.
[0048] The second step: Initiator preparation
[0049] Take 10Kg of ammonium persulfate, 3Kg of dibenzoyl peroxide (BPO), and 5Kg of distilled water into the mixing kettle, and stir thoroughly.
[0050] Step 3: Synthesize Acrylic Emulsion
[0051] Take 100Kg of acrylic acid and 100Kg of n-butyl acrylate and slowly add them to the reaction kettle of the first step in three times, stir well, control the temperature of the solution to keep 65-70°C, and keep it constant, then add 10Kg of the initiator mixed solution prepared in the second step , fully stirred for 150 minutes.
[0052...
Embodiment 2
[0057] With embodiment 1, difference is:
[0058] Step 1: Take 500Kg of distilled water, 10Kg of emulsifier OP-10, and 10Kg of sodium dodecylbenzenesulfonate.
[0059] Step 2: Take 20Kg of ammonium persulfate, 5Kg of dibenzoyl peroxide (BPO), and 10Kg of distilled water.
[0060] The third step: take 150Kg of acrylic acid, 150Kg of n-butyl acrylate, and 15Kg of initiator mixed solution.
[0061] The fourth step: take 50Kg acrylic acid emulsion synthesized in the third step, take 2Kg dispersant; Chromatic agent spiropyran, 0.6Kg water-based defoamer, 0.5Kg thickener, 8Kg ethyl acetate, 40Kg distilled water.
[0062] The performance of the product is as follows: 1. The appearance of the emulsion, the white emulsion is bluish; 2. The viscosity (25°C) is 180cp; 3. The hardness is 5H; 4. The appearance of the cured coating film is colorless, transparent, smooth and smooth; 5. Photochromic performance, Good reversible discoloration performance; 6. Anti-fatigue performance, 20W ultr...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com