[0028] Step 1: Dissolve 10 parts of aminating agent (6 parts of ammonia water, 3 parts of ethanolamine, 1 part of sodium hydroxide) in 150 parts of water, and heat to 70~80℃ for use;
[0029] Step 2: Add 12 parts of span-80, 4.5 parts of tween-80, 6 parts of op-10 emulsifier, 7.5 parts of sodium dodecylbenzene sulfonate and 2 parts of CMS stabilizer to 150 parts of water, and dissolve for later use;
[0030] Step 3: Add 11 parts of white oil, 15 parts of paraffin, 10 parts of stearic acid, and 15 parts of rosin to the reaction kettle, gradually increase the temperature to 80~90℃, start stirring, and slowly add to the step 1 standby after all the materials are melted Solution water, keep the temperature for 1.5 hours and cool down to about 40°C. Then add the solution of step two and stir evenly.
[0031] Step 4: Send the evenly stirred liquid to a sand mill for grinding, and the finished product is the finished product when the paraffin wax particles reach 3 to 5 μm to form a stable ...
Embodiment 2
[0033] Step 1: Dissolve 15 parts of aminating agent (9 parts of ammonia water, 3 parts of ethanolamine, 3 parts of sodium hydroxide) in 200 parts of water, and heat to 70~80℃ for standby;
[0034] Step 2: Add 14 parts of span-80, 7 parts of tween-80, 9 parts of op-10 emulsifier, 10 parts of sodium dodecylbenzene sulfonate and 1 part of stabilizer-polyacrylamide into 200 parts of water, and dissolve them for later use ;
[0035] Step 3: Add 15 parts of white oil, 20 parts of paraffin, 20 parts of stearic acid, and 20 parts of rosin to the reaction kettle, gradually increase the temperature to 80-90°C, start stirring, and slowly add to step 1 standby after all the materials are melted Solution water, keep the temperature for 1.5 hours and cool down to about 40°C. Then add the solution of step two and stir evenly.
[0036] Step 4: Send the evenly stirred liquid to a sand mill for grinding, and the finished product is the finished product when the paraffin wax particles reach 3 to 5 μm...
Embodiment 3
[0038] Step 1: Dissolve 9 parts of aminating agent (6 parts of ammonia water, 2.2 parts of ethanolamine, 0.8 parts of sodium hydroxide) in 100 parts of water, and heat to 70-80°C for use;
[0039] Step 2: Add 7 parts of span-80, 3 parts of tween-80, 5 parts of op-10 emulsifier, 5 parts of sodium dodecylbenzene sulfonate and 2 parts of CMC stabilizer to 100 parts of water, and dissolve for later use;
[0040] Step 3: Add 8 parts of white oil, 10 parts of paraffin, 8 parts of stearic acid, and 15 parts of rosin to the reaction kettle, gradually increase the temperature to 80~90℃, turn on the stirring, and slowly add to the step 1 standby after the materials are all melted Solution water, keep the temperature for 1.5 hours and cool down to about 40°C. Then add the solution of step two and stir evenly.
[0041] Step 4: Send the evenly stirred liquid to a sand mill for grinding, and the finished product is the finished product when the paraffin wax particles reach 3 to 5 μm to form a sta...