Reclaimed ABS (acrylonitrile butadiene styrene) environment-friendly modified material and preparation method thereof
A modified material and environmentally friendly technology, which is applied in the field of recycled ABS environmentally friendly modified materials and its preparation, can solve the problems of environmental damage and low mechanical properties, and achieve the effects of high purity, high gloss and enhanced flame retardancy of ABS
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0057] A recycled ABS environmentally friendly modified material, consisting of the following substances by weight:
[0058] ABS recycled material 100 copies
[0059] Flame retardant 5 parts
[0060] Flame retardant synergist 20 parts
[0061] Compound anti-aging agent 1 part
[0062] Antioxidant 0.4 parts
[0063] Toughener 10 parts
[0064] 2 parts of coupling agent.
[0065] The flame retardant is the modified graphene of the present invention.
[0066] The modified graphene is modified through the following methods:
[0067] (1) Put the graphene in absolute ethanol, and ultrasonically react for 1 hour to obtain a graphene suspension;
[0068] (2) After mixing deionized water, acetic acid with a mass concentration of 36%, and a silane coupling agent according to the mass percentage of 1:3:20, add it to the graphene suspension prepared in the first step, and continue the ultrasonic reaction for 20 minutes;
[0069] (3) Then keep the solution after the second step rea...
Embodiment 2
[0082] A recycled ABS environmentally friendly modified material, consisting of the following substances by weight:
[0083] ABS recycled material 100 copies
[0084] Flame retardant 8 parts
[0085] Flame retardant synergist 25 parts
[0086] Composite anti-aging agent 0.8 parts
[0087] Antioxidant 2 parts
[0088] Toughener 20 parts
[0089] 1 part of coupling agent.
[0090] The flame retardant is the modified graphene of the present invention.
[0091] The modified graphene is modified through the following methods:
[0092] (1) Put the graphene in absolute ethanol, and ultrasonically react for 1 hour to obtain a graphene suspension;
[0093] (2) After mixing deionized water, acetic acid with a mass concentration of 36%, and a silane coupling agent according to the mass percentage of 1:3:20, add it to the graphene suspension prepared in the first step, and continue the ultrasonic reaction for 20 minutes;
[0094] (3) Then keep the solution after the second step re...
Embodiment 3
[0107] A recycled ABS environmentally friendly modified material, consisting of the following substances by weight:
[0108] ABS recycled material 100 copies
[0109]Flame retardant 8 parts
[0110] Flame retardant synergist 18 parts
[0111] Composite anti-aging agent 0.5 parts
[0112] Antioxidant 1 part
[0113] Toughener 17 parts
[0114] 1.5 parts of coupling agent.
[0115] The flame retardant is the modified graphene of the present invention.
[0116] The modified graphene is modified through the following methods:
[0117] (1) Put the graphene in absolute ethanol, and ultrasonically react for 1.5 hours to obtain a graphene suspension;
[0118] (2) After mixing deionized water, acetic acid with a mass concentration of 36%, and a silane coupling agent according to the mass percentage of 1:3:20, add it to the graphene suspension prepared in the first step, and continue the ultrasonic reaction for 35 minutes;
[0119] (3) Then keep the solution after the second ste...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com