A kind of metal imitation button and preparation method thereof
A technology of imitating metal and buttons, applied in the field of garment production, can solve the problems of pollution of three wastes, single color effect, inability to achieve color, etc., and achieve the effect of low price and strong metal flashing luster.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
preparation example Construction
[0040] The invention discloses a method for preparing imitation metallic buttons, which is characterized in that it comprises the following steps:
[0041] A) After mixing the plastic raw materials, pigments, dispersants and pearlescent pigments, a blank-making mixture is obtained;
[0042] B) After the blanking mixture obtained in the above step A) is subjected to a forming process, an imitation metallic button is obtained.
[0043] In the above-mentioned preparation method of the present invention, the preferred principle and added amount of the raw materials used are consistent with the preferred principle and added amount in the aforementioned mixture, and will not be repeated here.
[0044] The present invention firstly mixes the plastic raw materials, the color material, the dispersant and the pearlescent pigment to obtain a blank-making mixture; the blank-making mixture is preferably a granular powder material.
[0045] The present invention has no particular limitation on the mi...
Embodiment 1
[0059] First, after stirring and mixing 800 g of PA, 5 g of powder organic colorant, 0.03 g of dispersant fatty acid polyethylene glycol ester, and 3 g of pearlescent pigment, mixing for 20 minutes to obtain a preformed particle powder mixture;
[0060] Then, put the granular powder mixture obtained in the above steps into the injection molding machine, combined with the mold made in the previous stage, under the conditions of a temperature of 240°C and an injection pressure of 750bar, the injection molding process is performed, and the injection molding of a mold product The time is 25 seconds, and finally the artificial imitation metal plastic button blank is obtained.
[0061] Finally, the button blank obtained in the above steps is subjected to subsequent button making processes such as hardening, cutting, polishing, and modeling, to obtain an imitation metal-plastic button.
[0062] Observe the artificial imitation metal buttons prepared by the above steps, see figure 1 , figure...
Embodiment 2
[0068] First, mix 1000g of ABS injection raw material, 4g of powdered organic colorant, 0.05g of dispersant fatty acid polyethylene glycol ester, and 5g of pearl pigment. After mixing for 25 minutes, a preformed particle powder mixture is obtained. ;
[0069] Then, put the granular powder mixture obtained in the above steps into the injection molding machine, combined with the mold made in the previous stage, and perform the injection molding process at a temperature of 200°C and an injection pressure of 800 bar. The injection molding of a mold product The time is 20 seconds, and finally the artificial imitation metal plastic accessories blank is obtained.
[0070] Finally, the accessory blanks obtained in the above steps are subjected to the subsequent hardening, cutting, polishing, modeling and other button making processes to obtain metal-plastic accessories.
[0071] Observe the artificial imitation metal accessories prepared by the above steps, see image 3 , image 3 This is t...