Oil painting pigment
A technology for oil paint and pigment powder, applied in the field of pigments, can solve the problems of unstable quality, high viscosity of oil paint, sticky pen, etc., and achieve the effects of improving shape retention ability, good emulsifying performance and saving materials
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] (1) Take linseed oil 2.9 and add it to the reaction kettle, set the temperature at 80°C, add white beeswax 1 and monoglyceride 1 while stirring, heat to 75°C, continue stirring for 20 minutes, wait for the white beeswax and monoglyceride All melted, released, and cooled for later use;
[0019] (2) Add 50% linseed oil into the material tank, add desiccant 0.1, barium sulfate 15%, pigment powder 30% while stirring at 200r / min, disperse at 400r / min for 20 minutes, add the semi-finished product obtained in step (1) , dispersed at a speed of 800 r / min until the surface of the slurry is smooth and free of particles, and then sent to a hydraulic grinder to grind to a fineness of less than 30 µm to obtain oil paint.
[0020] The pigment technical index that present embodiment makes:
[0021] Color difference (color difference meter) ΔE 0.98
[0022] Fineness (scraper fineness meter) 40µm
[0023] Tinting Power 102%
[0024] Density 1.5g / cm³
[0025] Covering Power 102%
...
Embodiment 2
[0030] (1) Add 2.85% linseed oil into the reaction kettle, set the temperature at 80°C, add white beeswax 2 and monoglyceride 2 while stirring, heat to 75°C, continue stirring for 20 minutes, wait for the white beeswax and monoglyceride All melted, released, and cooled for later use;
[0031] (2) Add linseed oil 20 into the material tank, add desiccant 0.15, barium sulfate 48, pigment powder 25 in turn while stirring at 200r / min, disperse at 400r / min for 20 minutes, add the semi-finished product obtained in step (1) , dispersed at a speed of 800 r / min until the surface of the slurry is smooth and free of particles, and then sent to a hydraulic grinder to grind to a fineness of less than 30 µm to obtain oil paint.
[0032] Technical indicators:
[0033] Color difference (color difference meter) ΔE 0.95
[0034] Fineness (scraper fineness meter) 39µm
[0035] Tinting Power 105%
[0036] Density 2.0g / cm³
[0037] Covering Power 105%
[0038] Lightfastness Class I
[0039] ...
Embodiment 3
[0042] (1) Take linseed oil 2.8 and add it to the reaction kettle, set the temperature at 80°C, add white beeswax 3 and monoglyceride 3 while stirring, heat to 75°C, continue stirring for 20 minutes, wait for the white beeswax and monoglyceride All melted, released, and cooled for later use;
[0043] (2) Add linseed oil 36 into the material tank, add desiccant 0.2, barium sulfate 50, pigment powder 5 in sequence while stirring at 200r / min, disperse at 400r / min for 20 minutes, add the semi-finished product obtained in step (1) , dispersed at a speed of 800 r / min until the surface of the slurry is smooth and free of particles, and then sent to a hydraulic grinder to grind to a fineness of less than 30 µm to obtain oil paint.
[0044] Technical indicators:
[0045] Color difference (color difference meter) ΔE 0.89
[0046] Fineness (scraper fineness meter) 39µm
[0047] Tinting Power 102%
[0048] Density 1.8g / cm³
[0049] Covering Power 102%
[0050] Lightfastness Class I ...
PUM
Property | Measurement | Unit |
---|---|---|
density | aaaaa | aaaaa |
density | aaaaa | aaaaa |
density | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com