Making method of coal gangue sintered brick
A manufacturing method and coal gangue technology, applied in the field of coal gangue sintered bricks, can solve the problems of uneven color of sintered bricks, insufficient sintering, environmental pollution, etc., and achieve the effects of energy saving, reasonable formula and simple operation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] Embodiment 1: a kind of manufacture method of coal gangue sintered brick,
[0019] Step 1: the component content is: 20 parts of coal gangue powder, 5 parts of cement, 3 parts of aluminum powder, 3 parts of gypsum, 2 parts of corundum mullite, 3 parts of saponin powder, 20 parts of fine sand, 8 parts of lime and The raw material particles of 8 parts of expanded perlite are broken into pulverized matter, and the particle diameter of described pulverized matter is fine powder of 60 meshes;
[0020] Step 2: Weigh each raw material according to the weight of the constituent raw materials, then mix the gangue with water and gypsum to make a slurry, then beat it into a slurry tank, heat it to 35°C, and then mix lime, cement, aluminum powder, and saponin Powder, fine sand, corundum mullite and expanded perlite are poured in and stirred for 5 minutes to obtain brick raw materials;
[0021] Step 3: Extrude the adobe raw material made in step 2 into adobe by hydraulic press, whe...
Embodiment 2
[0022] Embodiment 2: a kind of manufacture method of coal gangue sintered brick,
[0023] Step 1: the component content is: 25 parts of coal gangue powder, 8 parts of cement, 5 parts of aluminum powder, 4 parts of gypsum, 3 parts of corundum mullite, 4 parts of saponin powder, 22 parts of fine sand, 10 parts of lime and 10 parts of raw material particles of expanded perlite are broken into pulverized products, and the particle size of the pulverized products is a fine powder of 65 meshes;
[0024] Step 2: Weigh each raw material according to the weight of the constituent raw materials, then mix the gangue with water and gypsum to make a slurry, then beat it into a slurry tank, heat it to 40°C, and then mix lime, cement, aluminum powder, and saponin Powder, fine sand, corundum mullite and expanded perlite are poured in and stirred for 5 minutes to obtain brick raw materials;
[0025] Step 3: Extrude the adobe raw material made in step 2 into adobe by hydraulic press, wherein t...
Embodiment 3
[0026] Embodiment 3: a kind of manufacture method of coal gangue sintered brick,
[0027] Step 1: the component content is: 30 parts of coal gangue powder, 10 parts of cement, 8 parts of aluminum powder, 5 parts of gypsum, 5 parts of corundum mullite, 5 parts of saponin powder, 25 parts of fine sand, 12 parts of lime and 12 parts of raw material particles of expanded perlite are crushed into pulverized products, and the particle size of the pulverized products is a fine powder of 70 meshes;
[0028] Step 2: Weigh each raw material according to the weight of the constituent raw materials, then mix the coal gangue with water and gypsum to make a slurry, then beat it into a slurry tank, heat it to 45°C, and then mix lime, cement, aluminum powder, and saponin Powder, fine sand, corundum mullite and expanded perlite are poured in and stirred for 6 minutes to obtain brick raw materials;
[0029] Step 3: Extrude the adobe raw material produced in step 2 into adobe by hydraulic press...
PUM
| Property | Measurement | Unit |
|---|---|---|
| Particle size | aaaaa | aaaaa |
| Particle size | aaaaa | aaaaa |
| Particle size | aaaaa | aaaaa |