Waterborne environment-friendly epoxy zinc-rich primer and preparation method thereof

A technology of epoxy zinc-rich primer and water-based epoxy resin, applied in the field of paint, can solve the problems of blocking guns, unhealthy on-site personnel, polluting the environment, etc., and achieves good adaptability.

Inactive Publication Date: 2017-12-29
厦门日盛隆新材料科技有限公司
View PDF3 Cites 2 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

Disadvantages of 3-component waterborne epoxy zinc-rich coatings: ① The ratio of 3 components needs to be strictly controlled at the construction site
Zinc powder is mixed at the construction site, and the dust of zinc powder pollutes the environment, which is not good for the health of on-site personnel; ③ It takes a long time for zinc powder to disperse; It is easy to cause the gun to be blocked during spraying, which will affect the construction efficiency

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0020] A water-based environment-friendly epoxy zinc-rich primer, calculated by weight percentage, comprises the following components:

[0021] Water-based epoxy resin 47.4%, zinc powder 9.2%, zinc oxide 8.6%, phosphorus zinc white 0.6%, titanium dioxide 4.3%, sericite powder 0.6%, sodium selenite 0.43%, calcium carbonate 4.3%, talcum powder 4.3% , water 17.24%, ethylene glycol butyl ether 1.03%, dispersant 0.52%, wetting agent 0.25%, leveling agent 0.25%, defoamer 0.12%, thickener 0.52% and anti-settling agent 0.34%.

[0022] German Tego 760W as dispersant, German Tego 270 as wetting agent, German Tego 410 as leveling agent, German Tego 810 as defoamer, and Germany Tego 3030 as thickener.

[0023] Preparation:

[0024] 1) Mix titanium dioxide, sericite powder, zinc oxide, phosphorus-zinc white, sodium selenite, calcium carbonate, talcum powder, zinc powder and water and stir evenly for 30 minutes, then grind to obtain mixture A, finely The degree is 30 microns;

[0025] 2)...

Embodiment 2

[0027] A water-based environment-friendly epoxy zinc-rich primer, calculated by weight percentage, comprises the following components:

[0028] Waterborne epoxy resin 43.4%, zinc powder 9.2%, zinc oxide 8.6%, phosphorus zinc white 1.6%, titanium dioxide 4.3%, sericite powder 0.6%, sodium selenite 0.43%, calcium carbonate 5.3%, talcum powder 4.3% , water 19.24%, ethylene glycol butyl ether 1.03%, dispersant 0.52%, wetting agent 0.25%, leveling agent 0.25%, defoamer 0.12%, thickener 0.52% and anti-settling agent 0.34%.

[0029] German Tego 760W as dispersant, German Tego 270 as wetting agent, German Tego 410 as leveling agent, German Tego 810 as defoamer, and Germany Tego 3030 as thickener.

[0030] Preparation:

[0031] 1) Mix titanium dioxide, sericite powder, zinc oxide, phosphorus-zinc white, sodium selenite, calcium carbonate, talcum powder, zinc powder and water and stir evenly for 25 minutes, then grind to obtain mixture A, finely The degree is 35 microns;

[0032] 2) ...

Embodiment 3

[0034] A water-based environment-friendly epoxy zinc-rich primer, calculated by weight percentage, comprises the following components:

[0035] Water-based epoxy resin 49.4%, zinc powder 9.2%, zinc oxide 8.1%, phosphorus zinc white 0.6%, titanium dioxide 4.3%, sericite powder 0.6%, sodium selenite 0.43%, calcium carbonate 3.8%, talcum powder 4.3% , water 16.24%, ethylene glycol butyl ether 1.03%, dispersant 0.52%, wetting agent 0.25%, leveling agent 0.25%, defoamer 0.12%, thickener 0.52% and anti-settling agent 0.34%.

[0036] German Tego 760W as dispersant, German Tego 270 as wetting agent, German Tego 410 as leveling agent, German Tego 810 as defoamer, and Germany Tego 3030 as thickener.

[0037] Preparation:

[0038] 1) Mix titanium dioxide, sericite powder, zinc oxide, phosphorus-zinc white, sodium selenite, calcium carbonate, talcum powder, zinc powder and water and stir evenly for 35 minutes, then grind to obtain mixture A, finely The degree is 25 microns;

[0039] 2)...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention provides waterborne environment-friendly epoxy zinc-rich primer and a preparation method thereof. The waterborne environment-friendly epoxy zinc-rich primer is prepared from the following components by weight percent: 40 to 50 percent of waterborne epoxy resin, 15 to 20 percent of antirust agent, 10 to 15 percent of inorganic filler, 15 to 20 percent of water, 0.8 to 1.2 percent of co-solvent, 0.4 to 0.6 percent of dispersing agent, 0.2 to 0.3 percent of moisturizing agent, 0.2 to 0.3 percent of flatting agent, 0.1 to 0.16 percent of defoaming agent, 0.4 to 0.6 percent of thickening agent and 0.3 to 0.4 percent of anti-settling agent. The antirust agent is prepared from zinc powder, zinc oxide and zinc phosphate. The preparation method comprises the following steps: 1) uniformly mixing and stirring the antirust agent, the inorganic filler and the water, wherein the stirring time is 25 to 35 min, grinding, and obtaining a mixture A; and 2) adding waterborne epoxy resin into the mixture A, uniformly stirring for 25 to 35 min, then adding the co-solvent, the dispersing agent, the moisturizing agent, the flatting agent, the defoaming agent, the thickening agent and the anti-settling agent, and uniformly mixing, thus obtaining the waterborne environment-friendly epoxy zinc-rich primer. The primer is environmentally friendly, economical and good in antirust performance.

Description

technical field [0001] The invention belongs to the technical field of paints, and in particular relates to a water-based environment-friendly epoxy zinc-rich primer and a preparation method thereof. Background technique [0002] Traditional container coatings are mostly solvent-based coatings. Common varieties include epoxy, chlorinated rubber, acrylic, polyurethane, etc., which contain a large amount of organic solvents. These solvents are harmful to the health of construction workers and pollute the environment. Since the early 1970s, the development of environmentally friendly anti-corrosion and anti-rust paints such as high solid content, solvent-free, powder and water-based paints has been carried out in foreign countries. Among them, water-based paints have received more research because of their low cost, safe and convenient construction, and easy control of film thickness. . Due to the high technical difficulty, no major progress has been made for a long time. Sin...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
IPC IPC(8): C09D163/00C09D5/10C09D7/12
CPCC08K3/24C08K3/34C08K5/06C08K13/02C08K2003/0893C08K2003/2241C08K2003/2296C08K2003/265C08K2003/321C09D5/106C09D163/00
Inventor 张联良
Owner 厦门日盛隆新材料科技有限公司
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products