A technology of earthworms and red glaze, which is applied in the field of Jun porcelain manufacturing, can solve the problems of few formulas and preparation methods, low mechanical strength, and crystallization on the glaze surface, so as to enhance structural stability and mechanical strength, improve wear resistance, The effect of dense glaze layer
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] A copper red glaze with earthworm slime pattern, which is prepared from the following raw materials in parts by weight: 50-70 parts of feldspar, 12-18 parts of calcite, 8-12 parts of quartz, and 4-6 parts of copper ore , 5-7 parts of Suzhou soil, 2-4 parts of black wool soil, 0.5-1.5 parts of talc, 0.3-0.7 parts of copper oxide, 6-10 parts of zircon, and 6-10 parts of wollastonite.
[0023] The preparation method of the copper red glaze with earthworm slime pattern comprises the following steps:
[0024] (1) Crush the above raw materials and put them into a ball mill for ball milling, add water to make the mass concentration of the glaze reach 55-56%, wet mill for 8-10 hours, pass the wet milled slurry through a 120-300 mesh sieve to obtain glaze slurry ;
[0025] (2) The green body is dipped in glaze for 2-3 times;
[0026] (3) Firing, the firing temperature is 1280-1320°C.
[0027] In the present invention, the melamine feldspar is used as the main solvent, and the...
Embodiment 2
[0030] A copper red glaze with earthworm slime pattern, which is prepared from the following raw materials in parts by weight: 60 parts of feldspar, 15 parts of calcite, 10 parts of quartz, 5 parts of copper ore, 6 parts of Suzhou soil, black hair 3 parts of soil, 1 part of talc, 0.5 parts of copper oxide, 8 parts of zircon, and 8 parts of wollastonite.
[0031] The preparation method of the copper red glaze with earthworm slime pattern comprises the following steps:
[0032] (1) Crush the above raw materials and put them into a ball mill for ball milling, add water to make the mass concentration of the glaze reach 55-56%, wet mill for 8-10 hours, pass the wet milled slurry through a 120-300 mesh sieve to obtain glaze slurry ;
[0033] (2) The green body is dipped in glaze for 2-3 times;
[0034] (3) Firing, the firing temperature is 1280-1320°C.
[0035] It is characterized in that the firing process in step (3) specifically includes the following steps:
[0036] ①The bod...
Embodiment 3
[0041] A copper red glaze with earthworm slime pattern, which is prepared from the following raw materials in parts by weight: 60 parts of feldspar, 15 parts of calcite, 10 parts of quartz, 5 parts of copper ore, 6 parts of Suzhou soil, black hair 3 parts of soil, 1 part of talc, 0.5 parts of copper oxide, 8 parts of zircon, and 8 parts of wollastonite.
[0042] The preparation method of the copper red glaze with earthworm slime pattern comprises the following steps:
[0043] (1) Grind the above raw materials and put them into a ball mill for ball milling, add water to make the mass concentration of the glaze material reach 56%, wet mill for 9 hours, pass the wet milled slurry through a 200-mesh sieve to obtain the glaze slurry;
[0044] (2) The green body is dipped in glaze for 3 times;
[0045] (3) Firing, the firing temperature is 1300°C.
[0046] It is characterized in that the firing process in step (3) specifically includes the following steps:
[0047] ①The body afte...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com